Reversed copper foil with roughness of 1.0-1.5 [mu] m suitable for high-frequency field, preparation method and application
Through electrolytic preparation and surface treatment, the composition and treatment steps of electrolyte solution are optimized, and the problem of low peel strength of inverted copper foil is solved, and the inverted copper foil with low roughness and high peel strength is achieved. It is suitable for high-frequency and high-speed fields. copper clad and PCB board.
Patent Information
- Application Number
- CN202411039494.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
In the prior art, when preparing inverted copper foil with a roughness of 1.0≤Rz≤1.5μm, the peel resistance is low, resulting in poor production efficiency, complex management and high cost.
The raw foil is prepared by electrolysis and optimized by pickling, roughening, curing, anti-oxidation, passivation and silanization treatment, including Cu2+, sulfuric acid, Cl-, hydrolyzed collagen, tetrahydrothiazolethione and methylene Sodium bisnaphthalenesulfonate was roughened in two steps and cured three times to form dense copper tumors and improve the oxidation resistance of the copper foil.
Reverse copper foil with low roughness and high peel strength is achieved, suitable for the production of copper clad plates and PCB plates in high frequency and high speed fields. The peel strength is ≥0.85N/mm, the tensile strength is ≥350MPa, and the elongation is ≥6%. And tolerate baking at 200℃.
Smart Images

Figure CN118979290A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrolytic copper foil, and in particular to a reverse copper foil with a roughness of 1.0-1.5 μm suitable for high-frequency fields, a preparation method and an application thereof. Background Art
[0002] Electrolytic copper foil is one of the important components of copper-clad laminates and printed circuit boards, and plays a role in transmitting signals and electricity. The high-frequency and high-speed of signals makes signal transmission more and more concentrated on the "surface" of electrolytic copper foil, also known as the skin effect. For example, when the frequency reaches 1GHz, the transmission thickness of the signal on the surface of the electrolytic copper foil is about 2.1μm; when the signal transmission frequency is increased to 10GHz, the transmission thickness of the signal on the surface of the electrolytic copper foil is 0.70μm. If high-frequency and high-speed copper-clad laminates or printed circuit boards continue to use electrolytic copper foil with conventional roughness, the result is that as the signal transmission frequency increases, the signal "distortion" caused by the skin effect will become more serious.
[0003] In the prior art, in order to meet the demand for ultra-low profile copper foil in the high-frequency and high-speed fields, reverse electrolytic copper foil (RTF) is often used to prepare copper-clad laminates and PCB boards in the high-frequency and high-speed fields. Reverse electrolytic copper foil is a surface roughening treatment performed on the bonding surface between the electrolytic copper foil and the cathode roller. Since it is prepared using a low-roughness cathode roller, the smooth surface roughness of RTF copper foil is low, which reduces the cost of additives and has broad market prospects.
[0004] The relevant prior art specifically discloses a surface roughening and curing treatment method for RTF copper foil for high-frequency copper clad laminates, which specifically includes the following steps: step A, pickling pretreatment; step B, primary roughening electroplating: the original foil is electroplated in a roughening electrolytic cell using a pulse electroplating method, the forward and reverse time ratio of the pulse electroplating is 1:2 to 5:1, and the current density is guaranteed to be 20A to 100A / dm 2 ; Step C, primary weak solidification electroplating; Step D, repeat steps B and C 2 to 5 times; Step E, primary solidification electroplating: electroplate the original foil in a roughening electrolytic cell using a pulse electroplating method, with a forward and reverse time ratio of 3:1 to 10:1 for pulse electroplating, and a current density of 20A to 50A / dm 2 . The coating grains are refined, the surface is fine, and the oxidation resistance and corrosion resistance of the copper foil are improved. For example, Chinese patent CN116180163A discloses a method for manufacturing RTF copper foil, which includes an electrolytic raw foil step and a surface treatment step. The surface treatment step includes a roughening step, a curing step, and a silane treatment step. The roughening step includes a first roughening step. The first roughening step is to treat the copper foil obtained by the electrolytic raw foil step at a current density of 10 to 20 A / dm 2 Under the process parameters, H2SO4: 160 ~ 220g / L, Cu2+ :5~15g / L roughening solution electroplating roughening treatment, the roughening solution also adds WO4 2 : 170~250mg / L, C2H6O2·x: 300~400mg / L, C6H5O7 3 :75~145mg / L、MoO4 2 : 83 ~ 166mg / L and Cl: 20 ~ 40mg / L, which can ensure the bonding strength between the RTF copper foil and the matrix resin material while ensuring a low surface roughness value, thereby improving the peel strength of the bonding with the substrate.
[0005] However, so far, for RTF copper foil with a roughness of 1.0≤Rz≤1.5μm, the peel strength obtained by the existing technology is still relatively low, and for RTF copper foil with a peel strength ≥0.85N / mm, there are still problems such as poor production efficiency, complex production management and high production cost. In view of the problems existing in the existing technology, it is necessary to find a reverse copper foil with a roughness of 1.0-1.5μm suitable for high-frequency fields, a preparation method and application. Summary of the invention
[0006] In view of the problems existing in the prior art, the present invention provides a reverse copper foil with a roughness of 1.0-1.5 μm, which is suitable for the high-frequency field, a preparation method and an application thereof. The reverse copper foil of the present invention has both low roughness and high peeling strength, and is suitable for the production of copper-clad laminates and PCB boards in the high-frequency and high-speed fields.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] The present invention provides a method for preparing a reverse copper foil, comprising the following steps:
[0009] (1) Electrolytic preparation of raw foil: electrolyze a cathode roller with a roughness Rz ≤ 0.8 μm in an electrolyte to obtain raw foil;
[0010] The electrolyte includes: Cu 2+ , sulfuric acid, Cl - , hydrolyzed collagen, tetrahydrothiazolidinethione and sodium methylene bisnaphthalene sulfonate;
[0011] (2) Surface treatment: The smooth surface of the raw foil is pickled, roughened, cured, anti-oxidized, passivated and silanized, then dried and rolled.
[0012] Furthermore, the electrolyte includes: Cu 2+ 65-75g / L, sulfuric acid 90-100g / L, Cl -6-10mg / L, hydrolyzed collagen 50-70mg / L, tetrahydrothiazolidinethione 1-5mg / L and sodium methylene bisnaphthalene sulfonate 1-5mg / L.
[0013] Preferably, the electrolyte comprises Cu 2+ 70g / L, sulfuric acid 95g / L, Cl - 8mg / L, hydrolyzed collagen 60mg / L, tetrahydrothiazolidinethione 4mg / L and sodium methylene bisnaphthalene sulfonate 4mg / L.
[0014] Furthermore, the molecular weight of the hydrolyzed collagen is 5000-20000Da.
[0015] Furthermore, the electrolysis temperature in step (1) is 43-47° C., and the current is 25-30 kA.
[0016] Furthermore, the pickling in step (2) is carried out in a pickling solution having a sulfuric acid concentration of 130-150 g / L and a temperature of 40-44°C.
[0017] Furthermore, the roughening in step (2) includes a first roughening and a second roughening; the roughening solution 1 used in the first roughening includes 12-14 g / L Cu 2+ , 120-130g / L sulfuric acid, 0.02-0.04g / L Sn 2+ and 0.02-0.04 g / L Ti 4 + The second roughening solution 2 used in the roughening process includes 12-14 g / L Cu 2+ , 120-130g / L sulfuric acid and 0.2-0.4g / L sodium tungstate; the curing includes three curings, all of which are in Cu 2+ The oxidation prevention is carried out in a solution with a concentration of 60-70 g / L and a sulfuric acid concentration of 90-110 g / L; 2+ The concentration is 1.5-2.5g / L, Zn 2+ The passivation is carried out in a solution with a concentration of 3.5-4.5 g / L and a K4P2O7 concentration of 70-100 g / L; the passivation is carried out in a solution with a concentration of CrO4 2- The silanization is carried out in a solution with a silane concentration of 2.0-2.5 g / L and a K4P2O7 concentration of 70-100 g / L; the silanization is carried out in a solution with a silane concentration of 2.0-2.5 g / L.
[0018] Furthermore, the first roughening temperature is 30-34°C and the current density is 18A / dm 2 The second roughening temperature is 30-34 ° C, and the current density is 16A / dm 2The curing temperature is 45-50°C and the current density is 10A / dm 2 The anti-oxidation temperature is 35-45°C, the pH is 10-11, and the current density is 4.0A / dm 2 The passivation temperature is 20-30°C, the pH is 11-12, and the current density is 3.0A / dm 2 ; The silanization temperature is 30-40°C and the pH is 9-12.
[0019] Further, in step (1), Cl - Derived from HCl; Cu in steps (1) and (2) 2+ All are derived from copper sulfate; Sn in step (2) 2+ Derived from tin oxide and / or tin sulfate hydrate, the Ti 4+ Derived from titanium sulfate and / or titanium sulfate hydrate, the sodium tungstate is derived from sodium tungstate dihydrate; the Ni 2+ Derived from nickel sulfate and / or nickel sulfate hydrate, the Zn 2+ Derived from zinc sulfate and / or zinc sulfate hydrate, the CrO4 2- Derived from potassium dichromate and / or potassium dichromate hydrate; the silane includes one or more of KH550 silane coupling agent, KH560 silane coupling agent and KH570 silane coupling agent.
[0020] It is worth noting that the solvents used to prepare various solutions in the present invention are all ultrapure water.
[0021] Furthermore, the first roughening, the second roughening, the curing, the anti-oxidation and the passivation in step (2) all include a water washing step, wherein the water washing uses RO water at a temperature of 30-40°C.
[0022] Furthermore, the curing includes more than one curing, preferably three curings, and the parameter conditions of the three curings are consistent.
[0023] Furthermore, the drying in step (2) is carried out in an oven at a temperature of 105-125° C.; and the winding speed is 6-9 m / min.
[0024] Furthermore, the present invention also provides a reverse copper foil obtained by the above-mentioned preparation method.
[0025] Furthermore, the thickness of the reverse copper foil is 9-18 μm, and the roughness of the processed surface is: 1.0 μm≤Rz≤1.5 μm.
[0026] Furthermore, the reverse copper foil prepared by the above-mentioned preparation method or the above-mentioned reverse copper foil provided by the present invention can be used to prepare copper-clad laminates or PCB boards.
[0027] The technical effects achieved by the present invention are:
[0028] 1. The preparation method provided by the present invention can prepare a reverse copper foil of 9-18μm. First, a raw foil with a surface roughness of Rz≤1.0μm is prepared by electrolysis of raw foil, and then the impurities on the surface of the raw foil are removed by pickling of the surface treatment, and the copper foil is roughened twice and cured three times to obtain a copper nodule with small size, uniform shape, and firmly bonded to the raw foil surface; then both surfaces of the electrolytic copper foil are subjected to anti-oxidation, passivation, and silanization treatment to introduce high-temperature oxidation resistance and further improve the bonding force between the copper foil and the substrate. The resulting reverse copper foil has a thickness of 9-18μm and has the following characteristics: 1.0μm≤Rz≤1.5μm on the pressed surface, Rz≤2.5μm on the non-pressed surface, peel strength ≥0.85N / mm (characterized by FR4 substrate pressing test); tensile strength ≥350MPa, elongation ≥6%; no copper powder falls off after testing, and the copper foil surface can withstand oxidation discoloration after baking at 200℃ for 2h. It has both low roughness and high peel strength, and is suitable for the production of copper-clad laminates and PCB boards in high-frequency and high-speed fields.
[0029] 2. The present invention optimizes the electrolyte components and performs two-step roughening. First, dense and long copper nodules are formed by combining Ti and Sn ions. Then, tungstate ions are used to increase the roundness of the copper nodules, thereby making the copper nodules elliptical or conical, thereby improving the peel strength and comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic diagram of the process of the preparation method of the present invention;
[0031] Figure 2 This is the SEM image of the processed surface of the reverse copper foil prepared in Example 1. DETAILED DESCRIPTION
[0032] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0033] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are for describing specific embodiments rather than for limiting the scope of protection of the present invention.
[0034] When the embodiment gives a numerical range, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the present invention belongs.
[0035] The schematic diagram of the preparation method of the present invention is shown in Figure 1 .
[0036] It is worth noting that the raw materials used in the present invention are all common commercially available products, so their sources are not specifically limited.
[0037] Example 1
[0038] A method for preparing a reverse copper foil (taking 12 μm thickness as an example), specifically comprising the following steps:
[0039] (1) Electrolytic preparation of raw foil: electrolyze a cathode roller with a roughness Rz ≤ 0.8 μm in an electrolyte at a temperature of 45° C. and a current of 28 kA to obtain raw foil;
[0040] The electrolyte is specifically: Cu 2+ 70g / L, sulfuric acid 95g / L, Cl - 8mg / L, hydrolyzed collagen (molecular weight 10000Da) 60mg / L, tetrahydrothiazolidinethione 4mg / L and sodium methylene bisnaphthalene sulfonate 4mg / L;
[0041] (2) Surface treatment: The smooth surface of the raw foil is subjected to pickling, first roughening, water washing, second roughening, water washing, curing, water washing, anti-oxidation, water washing, passivation, water washing and silanization, and then dried and rolled in an oven at a temperature of 110°C at a rolling speed of 8m / min to obtain a reverse copper foil.
[0042] The pickling was carried out in a 140 g / L pickling solution at a temperature of 42°C;
[0043] The first roughening solution used was 13 g / L Cu 2+ , 125g / L sulfuric acid, 0.03g / L Sn 2+ and 0.03 g / L Ti 4+ , the roughening temperature is 32°C, the current density is 18A / dm 2 The second roughening solution used was 13 g / L Cu 2+ , 125g / L sulfuric acid and 0.3g / L sodium tungstate, the roughening temperature is 32℃, the current density is 16A / dm 2 ;
[0044] The curing was carried out three times, all in Cu2+ The curing temperature was 48℃ and the current density was 10A / dm 2 ;
[0045] Anti-oxidation in Ni 2+ The concentration is 2g / L, Zn 2+ The test was carried out in a solution with a concentration of 4 g / L and a K4P2O7 concentration of 80 g / L, with an anti-oxidation temperature of 40 °C, a pH of 10, and a current density of 4.0 A / dm 2 ;
[0046] Passivation in CrO4 2- The passivation temperature was 25°C, the pH was 11, and the current density was 3.0A / dm 2 ;
[0047] The silanization was carried out in a solution with a silane concentration of 2.0 g / L, a silanization temperature of 35° C., and a pH of 10.
[0048] The washing steps involved in step (2) all use RO water at a temperature of 35°C.
[0049] In step (1), Cl - All are derived from HCl; Cu in steps (1) and (2) 2+ All are derived from copper sulfate; Sn in step (2) 2+ Derived from tin oxide, Ti 4+ Derived from titanium sulfate, sodium tungstate is derived from sodium tungstate dihydrate; Ni 2+ From nickel sulfate, Zn 2+ From zinc sulfate, CrO4 2- Derived from potassium dichromate; silane is KH550 silane coupling agent.
[0050] The SEM image of the reverse copper foil treated surface prepared in Example 1 is shown in Figure 2 .
[0051] Example 2
[0052] A method for preparing a reverse copper foil (taking 12 μm thickness as an example), specifically comprising the following steps:
[0053] (1) Electrolytic preparation of raw foil: electrolyze a cathode roller with a roughness Rz ≤ 0.8 μm in an electrolyte at a temperature of 43° C. and a current of 25 kA to obtain raw foil;
[0054] The electrolyte is specifically: Cu 2+ 65g / L, sulfuric acid 90g / L, Cl -6mg / L, hydrolyzed collagen (molecular weight 5000Da) 50mg / L, tetrahydrothiazolidinethione 1mg / L and sodium methylene bisnaphthalene sulfonate 1mg / L;
[0055] (2) Surface treatment: The smooth surface of the raw foil is subjected to pickling, first roughening, water washing, second roughening, water washing, curing, water washing, anti-oxidation, water washing, passivation, water washing and silanization, and then dried and rolled in an oven at a temperature of 105°C at a rolling speed of 6m / min to obtain a reverse copper foil.
[0056] The pickling was carried out in a 130 g / L pickling solution at a temperature of 40°C;
[0057] The first roughening solution used was 12 g / L Cu 2+ , 120g / L sulfuric acid, 0.02g / L Sn 2+ and 0.02 g / L Ti 4+ , the roughening temperature is 30℃, the current density is 18A / dm 2 The second roughening solution used was 12 g / L Cu 2+ , 120g / L sulfuric acid and 0.2g / L sodium tungstate, the roughening temperature is 30℃, the current density is 16A / dm 2 ;
[0058] The curing was carried out three times, all in Cu 2+ The curing was carried out in solutions with a concentration of 60 g / L and 90 g / L sulfuric acid, the curing temperature was 45°C, and the current density was 10 A / dm 2 ;
[0059] Anti-oxidation in Ni 2+ The concentration is 1.5g / L, Zn 2+ The test was carried out in a solution with a concentration of 3.5 g / L and a K4P2O7 concentration of 70 g / L, with an anti-oxidation temperature of 35°C, a pH of 10, and a current density of 4.0 A / dm 2 ;
[0060] Passivation in CrO4 2- The passivation temperature was 20°C, the pH was 11, and the current density was 3.0A / dm 2 ;
[0061] The silanization was carried out in a solution with a silane concentration of 2.0 g / L, a silanization temperature of 30° C., and a pH of 9.
[0062] The washing steps involved in step (2) all use RO water at a temperature of 30°C.
[0063] In step (1), Cl - All are derived from HCl; Cu in steps (1) and (2) 2+ All are derived from copper sulfate; Sn in step (2) 2+ Derived from tin oxide, Ti 4+ Derived from titanium sulfate, sodium tungstate is derived from sodium tungstate dihydrate; Ni 2+ From nickel sulfate, Zn 2+ From zinc sulfate, CrO4 2- Derived from potassium dichromate; silane is KH560 silane coupling agent.
[0064] Example 3
[0065] A method for preparing a reverse copper foil (taking 12 μm thickness as an example), specifically comprising the following steps:
[0066] (1) Electrolytic preparation of raw foil: electrolyze a cathode roller with a roughness Rz ≤ 0.8 μm in an electrolyte at a temperature of 47° C. and a current of 30 kA to obtain raw foil;
[0067] The electrolyte is specifically: Cu 2+ 75g / L, sulfuric acid 100g / L, Cl - 10mg / L, hydrolyzed collagen (molecular weight 20000Da) 70mg / L, tetrahydrothiazolidinethione 5mg / L and sodium methylene bisnaphthalene sulfonate 5mg / L;
[0068] (2) Surface treatment: The smooth surface of the raw foil is subjected to pickling, first roughening, water washing, second roughening, water washing, curing, water washing, anti-oxidation, water washing, passivation, water washing and silanization, and then dried and rolled in an oven at a temperature of 125°C at a rolling speed of 9m / min to obtain a reverse copper foil.
[0069] The pickling was carried out in a 150 g / L pickling solution at a temperature of 44°C;
[0070] The first roughening solution used was 14 g / L Cu 2+ , 130g / L sulfuric acid, 0.04g / L Sn 2+ and 0.04 g / L Ti 4+ , the roughening temperature is 34°C, the current density is 18A / dm 2 The second roughening solution used was 14 g / L Cu 2+ , 130g / L sulfuric acid and 0.4g / L sodium tungstate, the roughening temperature is 34℃, the current density is 16A / dm 2 ;
[0071] The curing was carried out three times, all in Cu 2+The curing was carried out in solutions with a concentration of 70 g / L and a concentration of 110 g / L sulfuric acid, the curing temperature was 50 °C, and the current density was 10 A / dm 2 ;
[0072] Anti-oxidation in Ni 2+ The concentration is 2.5g / L, Zn 2+ The test was carried out in a solution with a concentration of 4.5 g / L and a K4P2O7 concentration of 100 g / L, with an anti-oxidation temperature of 45°C, a pH of 11, and a current density of 4.0 A / dm 2 ;
[0073] Passivation in CrO4 2- The passivation temperature was 30°C, the pH was 12, and the current density was 3.0A / dm 2 ;
[0074] The silanization was carried out in a solution with a silane concentration of 2.5 g / L, a silanization temperature of 40° C., and a pH of 12.
[0075] The washing steps involved in step (2) all use RO water at a temperature of 40°C.
[0076] In step (1), Cl - All are derived from HCl; Cu in steps (1) and (2) 2+ All are derived from copper sulfate; Sn in step (2) 2+ Derived from tin oxide, Ti 4+ Derived from titanium sulfate, sodium tungstate is derived from sodium tungstate dihydrate; Ni 2+ From nickel sulfate, Zn 2+ From zinc sulfate, CrO4 2- Derived from potassium dichromate; silanes include KH570 silane coupling agent.
[0077] Comparative Example 1
[0078] The only difference from Example 1 is that the hydrolyzed collagen and tetrahydrothiazolidinethione are replaced by an equal amount of sodium methylenebisnaphthalenesulfonate, that is, the electrolyte is specifically: Cu 2+ 70g / L, sulfuric acid 95g / L, Cl - 8mg / L and sodium methylene bisnaphthalene sulfonate 68mg / L.
[0079] Comparative Example 2
[0080] The only difference from Example 1 is that the hydrolyzed collagen and sodium methylene bisnaphthalene sulfonate are replaced by an equal amount of tetrahydrothiazolidinethione, that is, the electrolyte is specifically: Cu 2+ 70g / L, sulfuric acid 95g / L, Cl -8mg / L and tetrahydrothiazolidinethione 68mg / L.
[0081] Comparative Example 3
[0082] The only difference from Example 1 is that tetrahydrothiazolidinethione and sodium methylene bisnaphthalene sulfonate are replaced by an equal amount of hydrolyzed collagen, that is, the electrolyte is specifically: Cu 2+ 70g / L, sulfuric acid 95g / L, Cl - 8mg / L and hydrolyzed collagen (molecular weight 10000Da) 68mg / L.
[0083] Comparative Example 4
[0084] The only difference from Example 1 is that the roughening step is performed only once (the roughening solution is the combination of two roughening solutions), that is, specifically, the following steps:
[0085] (1) Electrolytic preparation of raw foil: electrolyze a cathode roller with a roughness Rz ≤ 0.8 μm in an electrolyte at a temperature of 45° C. and a current of 28 kA to obtain raw foil;
[0086] The electrolyte is specifically: Cu 2+ 70g / L, sulfuric acid 95g / L, Cl - 8mg / L, hydrolyzed collagen (molecular weight 10000Da) 60mg / L, tetrahydrothiazolidinethione 4mg / L and sodium methylene bisnaphthalene sulfonate 4mg / L;
[0087] (2) Surface treatment: The smooth surface of the raw foil is pickled, roughened, washed, cured, washed, anti-oxidized, washed, passivated, washed and silanized, and then dried and rolled in an oven at a temperature of 110°C at a rolling speed of 8m / min to obtain a reverse copper foil.
[0088] The pickling was carried out in a 140 g / L pickling solution at a temperature of 42°C;
[0089] The roughening solution used for roughening is 16g / L Cu 2+ , 250g / L sulfuric acid, 0.03g / L Sn 2+ and 0.03g / L Ti 4+ and 0.3g / L sodium tungstate, the roughening temperature is 32℃, the current density is 18A / dm 2 ;
[0090] The curing was carried out three times, all in Cu 2+ The curing temperature was 48℃ and the current density was 10A / dm 2 ;
[0091] Anti-oxidation in Ni2+ The concentration is 2g / L, Zn 2+ The test was carried out in a solution with a concentration of 4 g / L and a K4P2O7 concentration of 80 g / L, with an anti-oxidation temperature of 40 °C, a pH of 10, and a current density of 4.0 A / dm 2 ;
[0092] Passivation in CrO4 2- The passivation temperature was 25°C, the pH was 11, and the current density was 3.0A / dm 2 ;
[0093] The silanization was carried out in a solution with a silane concentration of 2.0 g / L, a silanization temperature of 35° C., and a pH of 10.
[0094] The washing steps involved in step (2) all use RO water at a temperature of 35°C.
[0095] In step (1), Cl - All are derived from HCl; Cu in steps (1) and (2) 2+ All are derived from copper sulfate; Sn in step (2) 2+ Derived from tin oxide, Ti 4+ Derived from titanium sulfate, sodium tungstate is derived from sodium tungstate dihydrate; Ni 2+ From nickel sulfate, Zn 2+ From zinc sulfate, CrO4 2- Derived from potassium dichromate; silane is KH550 silane coupling agent.
[0096] Physical specific tests were performed on the reverse copper foils obtained in the embodiments and comparative examples. The physical property test items and methods were as follows:
[0097] A. Roughness: Refer to GB / T 5230-2020 Electrolytic Copper Foil for Printed Boards and test with a roughness meter.
[0098] B. Peel strength: Refer to GB / T 5230-2020 Electrolytic Copper Foil for Printed Boards. After FR4 prepreg lamination, peel test is performed using a universal mechanical testing machine.
[0099] C.Tensile strength and elongation at room temperature: refer to GB / T 5230-2020 Electrolytic copper foil for printed boards and use a universal mechanical testing machine for tensile testing.
[0100] D. Copper powder shedding: Place the rough surface of the filter paper in contact with the rough cured surface of the copper foil, place a 200g weight on the other side of the filter paper, drag the filter paper evenly for 50cm, observe the copper powder on the rough surface of the filter paper, and determine the grade. (Evaluation criteria for powder shedding: Grade O: no copper powder shedding, Grade 1: a small amount of copper powder shedding, Grade 2:
[0101] Copper powder obviously falls off).
[0102] E. Antioxidation: Refer to GB / T 5230-2020 Electrolytic Copper Foil for Printed Boards and test in an oven that can provide 250°C.
[0103] The results are shown in the following table:
[0104] Table 1 Physical specific results of the reverse copper foil of the present invention
[0105]
[0106] According to the results in the above table, the reverse copper foil in the present invention has the following characteristics: the lamination surface is 1.0μm≤Rz≤1.5μm, the non-lamination surface is Rz≤2.5μm, the peel strength is ≥0.85N / mm (characterized by the FR4 substrate lamination test), the tensile strength is ≥350MPa, and the elongation is ≥6%. After testing, no copper powder falls off, and the copper foil surface can withstand oxidation and discoloration after baking at 200℃ for 2h. It has both low roughness and high peel strength, and is suitable for the production of copper-clad laminates and PCB boards in high-frequency and high-speed fields.
[0107] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a reverse copper foil, characterized in that: The following steps are involved: (1) Electrolytic preparation of raw foil: electrolyze a cathode roller with a roughness Rz ≤ 0.8 μm in an electrolyte to obtain raw foil; The electrolyte includes: Cu 2+ , sulfuric acid, Cl - , hydrolyzed collagen, tetrahydrothiazolidinethione and sodium methylene bisnaphthalene sulfonate; (2) Surface treatment: The smooth surface of the raw foil is pickled, roughened, cured, anti-oxidized, passivated and silanized, then dried and rolled.
2. The preparation method according to claim 1, characterized in that: The electrolyte includes: Cu 2+ 65-75g / L, sulfuric acid 90-100g / L, Cl - 6-10mg / L, hydrolyzed collagen 50-70mg / L, tetrahydrothiazolidinethione 1-5mg / L and sodium methylene bisnaphthalene sulfonate 1-5mg / L.
3. The preparation method according to claim 1, characterized in that: The molecular weight of the hydrolyzed collagen is 5000-20000Da.
4. The preparation method according to claim 1, characterized in that: The electrolysis temperature in step (1) is 43-47° C. and the current is 25-30 kA.
5. The preparation method according to claim 1, characterized in that: The pickling in step (2) is carried out in a pickling solution having a sulfuric acid concentration of 130-150 g / L and a temperature of 40-44°C.
6. The preparation method according to claim 1, characterized in that: The roughening in step (2) includes a first roughening and a second roughening; the roughening solution 1 used in the first roughening includes 12-14 g / L Cu 2+ , 120-130g / L sulfuric acid, 0.02-0.04g / L Sn 2+ and 0.02-0.04 g / L Ti 4+ The second roughening solution 2 used in the roughening process includes 12-14 g / L Cu 2+ , 120-130g / L sulfuric acid and 0.2-0.4g / L sodium tungstate; the curing includes three curings, all of which are in Cu 2+ The oxidation prevention is carried out in a solution with a concentration of 60-70 g / L and a sulfuric acid concentration of 90-110 g / L; 2+ The concentration is 1.5-2.5g / L, Zn 2 + The passivation is carried out in a solution with a concentration of 3.5-4.5 g / L and a K4P2O7 concentration of 70-100 g / L; the passivation is carried out in a solution with a concentration of CrO4 2- The silanization is carried out in a solution with a silane concentration of 2.0-2.5 g / L and a K4P2O7 concentration of 70-100 g / L; the silanization is carried out in a solution with a silane concentration of 2.0-2.5 g / L.
7. The preparation method according to claim 6, characterized in that: The first roughening temperature is 30-34°C and the current density is 18A / dm 2 The second roughening temperature is 30-34 ° C, and the current density is 16A / dm 2 The curing temperature is 45-50°C and the current density is 10A / dm 2 The anti-oxidation temperature is 35-45°C, the pH is 10-11, and the current density is 4.0A / dm 2 The passivation temperature is 20-30°C, the pH is 11-12, and the current density is 3.0A / dm 2 ; The silanization temperature is 30-40°C and the pH is 9-12.
8. The preparation method according to claim 6, characterized in that: In step (1), Cl - Derived from HCl; Cu in steps (1) and (2) 2+ All are derived from copper sulfate; Sn in step (2) 2+ Derived from tin oxide and / or tin sulfate hydrate, the Ti 4+ Derived from titanium sulfate and / or titanium sulfate hydrate, the sodium tungstate is derived from sodium tungstate dihydrate; the Ni 2+ Derived from nickel sulfate and / or nickel sulfate hydrate, the Zn 2+ Derived from zinc sulfate and / or zinc sulfate hydrate, the CrO4 2- Derived from potassium dichromate and / or potassium dichromate hydrate; the silane includes one or more of KH550 silane coupling agent, KH560 silane coupling agent and KH570 silane coupling agent.
9. The reverse copper foil obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the reverse copper foil prepared by the preparation method according to any one of claims 1 to 8 or the reverse copper foil according to claim 9 in preparing copper clad laminates or PCBs.
Citation Information
Patent Citations
Surface roughening and curing treatment method of RTF copper foil for high-frequency copper-clad plate
CN112921371A
RTF copper foil manufacturing method
CN116180163A
Cited By
Preparation method and application of electronic foil capable of providing high response