Environment-friendly high-insulation profile steel paper as well as slurry composition and preparation method thereof
By using slurry compositions of degreased cotton fibers and wood pulp fibers, high-insulating steel paper was prepared, which solved the shortcomings of existing steel paper in terms of environmental protection and insulation performance, achieved the improvement of high density and high insulation performance, and met the satisfaction of Modern performance requirements.
Patent Information
- Application Number
- CN202411466749.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-21
- Publication Date
- 2024-11-19
AI Technical Summary
Existing steel paper has shortcomings in environmental protection and insulation properties, especially when using natural fibers, it is difficult to meet modern performance requirements, and traditional glass fiber materials have shortcomings in environmental protection.
The slurry composition is made of 90-95% long fiber and 5-10% short fiber, wherein the long fiber is defatted cotton fiber and the short fiber is wood pulp fiber. The high is prepared by pulping, dilution, purification, heating and pressurization. Insulated steel paper, avoid using inorganic fibers.
The steel paper products with environmentally friendly and high insulation performance have better performance than traditional steel paper, significantly improved density and insulation strength, and used environmentally friendly plant-derived raw materials.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of special paper, and in particular to environmentally friendly high-insulation steel paper and a slurry composition and a preparation method thereof. Background Art
[0002] Steel paper is a special kind of paper. It is made of cellulose and its derivatives as raw materials. It uses metal salts that have strong swelling and gelling properties on cellulose as treating agents. The steel paper base paper is treated and laminated to produce modified processed paper.
[0003] Glass fiber is an inorganic non-metallic material with excellent performance, and has the advantages of good insulation, strong heat resistance, good corrosion resistance and high mechanical strength. Therefore, it is used as one of the raw materials of steel paper. For example, CN103103867A discloses a steel paperboard, which is made of 94%-97% by weight of absorbent cotton fiber and 3%-6% by weight of glass fiber. Another example is the glass fiber composite steel paper disclosed in CN210132411U, which is composed of a steel paper body and a glass fiber layer. However, with the advancement of science and technology and the improvement of people's awareness of environmental protection, more environmentally friendly raw materials are needed to replace glass fiber.
[0004] In addition, fibers from natural sources are also widely used as raw materials for steel paper. Although fibers from natural sources are more environmentally friendly, they are not good enough when processed into steel paper and cannot meet the increasingly high performance requirements of modern society for products. For example, when using only natural fibers such as plant fibers, there are problems with high insulation performance and tensile strength. There is still a demand for more environmentally friendly and higher performance steel paper products.
[0005] The information in the background technology is only for illustrating the general background of the present invention and should not be regarded as admitting or suggesting in any form that such information constitutes the prior art known to a person skilled in the art. Summary of the invention
[0006] In order to solve at least some of the technical problems in the prior art, the present invention provides environmentally friendly and highly insulating steel paper and its slurry composition and preparation method. Specifically, the present invention includes the following contents.
[0007] The first aspect of the present invention provides an environmentally friendly high-insulation steel paper pulp composition, which includes 90-95 parts by weight of long fibers and 5-10 parts by weight of short fibers, wherein the long fibers are cotton wool fibers with a length of 2-25 mm, the short fibers are wood pulp fibers with a length of 1-2 mm, and the long fibers and the short fibers are each hydrophilic fibers, and the pulp composition does not contain inorganic fibers.
[0008] In certain embodiments, according to the environmentally friendly high-insulation steel pulp composition of the present invention, the Kappa number of the wood pulp fiber is 5-20.
[0009] In certain embodiments, according to the environmentally friendly high-insulation steel pulp composition of the present invention, the inorganic fibers include glass fibers.
[0010] A second aspect of the present invention provides a method for preparing an environmentally friendly high-insulation steel paper, which comprises the following steps: (1) the pulp composition described in the first aspect is passed into a pulping machine for pulping, then passed into a stock preparation box for mixing, further subjected to dilution and / or purification, and subjected to dehydration treatment in a papermaking machine to form a wet paper web, and the water content is controlled within the range of 4-8% by pressing and drying to obtain steel paper base paper; (2) soaking the multi-layer steel paper in a solution for 1-10 minutes, wherein the solution is a 50-88 wt % zinc chloride solution; (3) heating and pressurizing the soaked multi-layer steel paper base paper to form a semi-finished product; (4) The product is aged at 20-40°C, desalted and dried to obtain environmentally friendly high-insulation steel paper.
[0011] In certain embodiments, the method for preparing the environmentally friendly high-insulation steel paper according to the present invention further comprises a step of adjusting the short fiber Kappa number to 5-20 before step (1).
[0012] In certain embodiments, according to the method for preparing environmentally friendly high-insulation steel paper of the present invention, the beating degree in step (1) is 15-25°SR, and the wet weight is 8-18g.
[0013] In certain embodiments, the method for preparing the environmentally friendly high-insulation steel paper according to the present invention further comprises a step of shaping by a calender after step (4).
[0014] The third aspect of the present invention provides an environmentally friendly high-insulation steel paper, which is prepared using the slurry composition described in the first aspect or prepared by the method described in the second aspect.
[0015] In certain embodiments, the environmentally friendly high-insulation steel paper according to the present invention has a thickness of 0.02-5 mm and a density of 1-2.5 kg / dm 3 .
[0016] The steel paper pulp composition of the present invention uses plant-derived fibers as raw materials, and it is found that long fibers are mainly used, and supplementing with an appropriate amount of short fibers is more conducive to the combination of different fibers, thereby providing environmentally friendly products while basically maintaining the performance of inorganic fiber materials, or even better. DETAILED DESCRIPTION
[0017] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0018] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that the upper and lower limits of the scope and each intermediate value therebetween are specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0019] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as commonly understood by those skilled in the art to which the invention belongs. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0020] In this article, the term "steel paper", sometimes also called "hardened paper" or "paper steel", refers to a high-hardness special paper made of fiber material. It has excellent elasticity, toughness, wear resistance and corrosion resistance, as well as good electrical insulation and mechanical strength. It can be used as mechanical parts such as gaskets.
[0021] Herein, the term "slurry composition", sometimes referred to as "slurry" or "paper stock", is a fibrous substance obtained by processing. Generally, the slurry composition further includes water to form a mixture. According to the fiber components of the slurry, the slurry is divided into plant fiber slurry, such as wood pulp (or wood fiber pulp), grass pulp (herbaceous plants such as stem fiber pulp), or inorganic material fiber slurry, such as glass fiber pulp. Generally, the slurry composition is a mixture containing multiple fibers, wherein inorganic material fibers are usually used as supplementary fibers.
[0022] Herein, the term "length", when used as a fiber characteristic, generally refers to the fiber length of the initial raw material, especially the average length. During the pulp processing, different processing conditions may cause different degrees of degradation, shortening, etc. of the length of the initial raw material fiber.
[0023] [Steel pulp composition] In a first aspect of the present invention, there is provided an environmentally friendly high-insulation steel paper pulp composition, which comprises two fibers of different lengths, namely long fibers and short fibers, preferably, the short fibers have a harderness than the long fibers. The present invention finds that when the long fibers and the short fibers are respectively hydrophilic fibers, preferably the hydrophilic properties of the two fibers are the same or similar, it is more conducive to promoting the combination of the two different fibers, thereby improving the tensile strength of the steel paper.
[0024] Long Fiber The long fiber of the present invention refers to a fiber having a longer length relative to another fiber in the steel-paper pulp composition. The length of the long fiber is generally controlled within the range of 2-25 mm, such as 3 mm, 5 mm, 6 mm, 8 mm, 10 mm, 12 mm, 15 mm, 16 mm, 18 mm, 20 mm, 22 mm, and 24 mm. Those skilled in the art will appreciate that the above length range is only exemplary, and other suitable lengths may be selected as required, such as 26 mm, 27 mm, 28 mm, 29 mm, 30 mm, etc. Preferably, the long fiber of the present invention is a flexible fiber, that is, it is more flexible than the short fiber.
[0025] In the present invention, the amount of the long fibers is 90 to 95 parts by weight, such as 91 parts by weight, 92 parts by weight, 93 parts by weight, 94 parts by weight, and 95 parts by weight. When the amount of the long fibers is within the above range, the contact between the long fibers can be ensured, while the regulating effect of the short fibers can be fully exerted.
[0026] In the present invention, the long fiber is absorbent cotton fiber. Compared with non-absorbent cotton fiber, the combination of absorbent cotton fiber and the short fiber of the present invention can further improve the insulation performance of the steel paper fiber. The reason is unclear and is not bound by theoretical explanation. The possible reason is that the absorbent cotton fiber has a higher hydrophilicity, which is equivalent to the hydrophilicity of the short fiber, especially the wood pulp fiber, which is conducive to the combination of the fibers during hot pressing, improves the strength, and then improves the insulation.
[0027] Short Fiber The length of the staple fibers of the present invention is generally selected in the range of 1-2 mm. In certain embodiments, the length of the staple fibers of the present invention is 1 / 3 to 1 / 10 of the length of the long fibers, such as 1 / 4, 1 / 5, 1 / 6, 1 / 7, 1 / 8, 1 / 9, etc.
[0028] In the present invention, preferably, the short fibers have a higher hardness, which may also be referred to as hard fibers, so that when forming steel paper pulp, the hard fibers can be randomly dispersed among a plurality of long fibers and promote bonding between the fibers during subsequent processing.
[0029] In the present invention, the amount of the short fibers is 5-10 parts by weight, such as 6 parts by weight, 7 parts by weight, 8 parts by weight, and 9 parts by weight. When the amount of the short fibers is within the above range, the short fibers can give full play to the hardness of the short fibers without affecting the bonding between the long fibers. If the amount of the short fibers is too high, the short fibers tend to be dispersed in large quantities between the long fibers, which is not conducive to improving the contact and bonding between the long fibers, affecting the toughness of the steel paper. On the other hand, if the amount is too low, the long fibers tend to be excessively contacted, which is not conducive to improving the hardness of the steel paper.
[0030] In certain embodiments, the short fibers of the present invention are wood pulp fibers. That is, fibers made from woody plants as raw materials. Wood pulp fibers can be virgin wood pulp, recycled wood pulp, or a mixture of the two in any proportion. The type of woody plant used as the raw material is not limited, and any woody plant known in the art can be selected, and examples thereof include but are not limited to broad-leaved plants such as birch, poplar, basswood, eucalyptus, maple, and coniferous plants such as fish-scale spruce, sand pine spruce, stinking fir, Korean pine, larch, and masson pine.
[0031] In certain embodiments, the wood pulp fiber of the present invention preferably has a kappa number of 5-20, such as 6, 7, 8, 9, 10, 12, 14, 15, 16, 18, etc. The present invention has found that when the kappa number is within the above range, the insulation performance of the steel paper produced can be greatly improved, and the density is higher. If the kappa number is too high, the insulation performance of the steel paper tends to decrease significantly.
[0032] [Method for preparing steel paper] A second aspect of the present invention provides a method for preparing an environmentally friendly high-insulation steel paper, which includes but is not limited to the following steps: (1) the slurry composition is passed into a pulping machine for pulping, then passed into a stock preparation box for mixing, further diluted and / or purified, and dehydrated by a paper machine to form a wet paper web, and the water content is controlled within a range of 4-8% by pressing and drying to obtain steel paper base paper; (2) soaking the multi-layer steel paper in a solution for 1-10 minutes, wherein the solution is a 50-88 wt % zinc chloride solution; (3) heating and pressurizing the soaked multi-layer steel paper base paper to form a semi-finished product; (4) The product is aged at 20-40°C, desalted and dried to obtain environmentally friendly high-insulation steel paper.
[0033] Those skilled in the art will appreciate that the numbers (1), (2), etc. herein are only for the purpose of distinguishing different steps and do not indicate the order of the steps. As long as the purpose of the present invention can be achieved, the order of the above steps is not particularly limited. In addition, two or more of the above steps may be combined or performed simultaneously. In addition, those skilled in the art will appreciate that other steps or operations may be included before or after the above steps (1)-(4), or between these arbitrary steps, such as further optimizing and / or improving the method described in the present invention. For example, optionally, the present invention further comprises: (5) before step (1), further comprising the step of adjusting the kappa number of the short fibers to 5-20; (6) After step (4), the step of further shaping by a calender is included.
[0034] Step (1) Step (1) of the present invention is a step for obtaining steel paper base paper, specifically, comprising allowing the pulp composition to enter a pulping machine for pulping treatment, then enter a pulping box for mixing, further undergoing dilution and / or purification treatment, and undergoing dehydration treatment through a papermaking machine to form a wet paper web, and controlling the water content in the range of 4-8% through pressing and drying to obtain steel paper base paper.
[0035] In the present invention, beating is performed in a pulping machine to increase the flexibility and interweaving of the fibers. The beating can be performed using a disc refiner, a conical refiner, or the like. The beating degree is controlled to be 15-25°SR, such as 16, 18, 20, 22, 24°SR; the wet weight is 8-18g, such as 9, 10, 12, 14, 16g, or the like. When preparing the slurry, the slurry is diluted to a solid content of 40-60% by weight. The purification treatment is used to remove fine impurities and particles. The purification method is not limited, and can be performed by, for example, precipitation, filtration, or flotation. Precipitation is the process of causing impurities to settle to the bottom by gravity. Filtration is the process of using filter media such as filter cloth or filter screen to intercept impurities. Flotation is the process of using bubbles to bring impurities to the surface of the slurry and remove them. The present invention can use any of the above methods or a combination of multiple methods for purification.
[0036] In the present invention, dehydration is a process of removing moisture from a mesh by vacuum to form wet paper. Pressing in the present invention further removes moisture. After pressing, the paper is transferred from the wet mesh to a wet machine, where heat transfer is used to achieve the purpose of drying, and then hot air drying is used to form base paper. In the present invention, the wet mesh can reduce the damage to the wet paper during the transfer process and maintain the flatness of the paper. The wet paper undergoes a wetting process on the wet mesh, which makes the cellulose fibers more tightly bonded, which is beneficial to the heat transfer effect in the subsequent drying process.
[0037] Next, the purpose of drying is achieved through heat transfer in a wet machine. The wet machine is the main equipment used for paper drying. The wet paper is heated by hot rollers and hot air to evaporate the moisture in the paper. In the wet machine, the wet paper is sent into the pressing area between the hot rollers. Under high pressure and high temperature, the moisture is squeezed out of the paper, making the surface of the paper dry. At the same time, the hot air heats the paper to increase the heat transfer effect and speed up the paper drying.
[0038] Step (2) Step (2) of the present invention is a gelling treatment step, specifically, comprising soaking the multi-layer steel paper base paper in a chemical solution for 1-10 minutes, such as 1 minute, 2 minutes, 2.5 minutes, 3 minutes, 3.5 minutes, etc.
[0039] In the present invention, gelation is performed in a gelation tank, and the temperature during gelation is not limited, for example, immersion gelation can be performed within the range of 15-40°C. Exemplary gelation temperatures include room temperature, 30°C, 35°C, 36°C, etc. The concentration of the medicine used in the present invention is generally 50-88% by weight of zinc chloride solution, preferably, the concentration of zinc chloride is 55% by weight, 60% by weight, 62% by weight, 64% by weight, 65% by weight, 68% by weight, 70% by weight, 75% by weight, 80% by weight, 85% by weight, etc.
[0040] Step (3) Step (3) of the present invention is a step for preparing a semi-finished product, specifically, comprising heating and pressurizing the soaked multi-layer steel paper base paper to form a strong bond between the layers. Heating and pressurizing can be performed separately or simultaneously. Heating and pressurizing at the same time is more conducive to the bonding between the base paper layers, and is therefore preferred. The heating temperature of the present invention is generally 30-90°C, for example, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, etc. When heating at high temperature, it is preferred to heat under wet conditions. The pressurization of the present invention is generally performed by a pressure roller, and the pressure size is not limited.
[0041] Step (4) The step (4) of the present invention is an aging and desalting treatment step, which includes aging treatment at 20-40°C, desalting treatment, and drying to obtain environmentally friendly high-insulation steel paper.
[0042] In the present invention, the aging treatment is carried out in an aging furnace, and the aging temperature is generally controlled at 25-40°C, such as 30°C, 32°C, 25°C, etc. The aging time is generally 30-120 minutes, such as 40 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes, 90 minutes, etc. The aging time is generally related to the aging temperature. Generally, when the aging temperature is low, the aging treatment time is appropriately extended.
[0043] In the present invention, the desalination treatment includes allowing the steel paper to enter a plurality of cleaning tanks with gradually decreasing concentrations and finally pure water for desalination treatment, and the zinc chloride concentrations in the cleaning tanks are 60%, 30%, 15%, 8%, 4%, 2%, 1%, 0.5%, 0.05%, and 0. The desalination treatment time of each cleaning tank is controlled within 20-60 minutes, thereby making the surface of the steel paper smoother and more delicate. The steel paper is dried.
[0044] [Environmentally friendly high insulation steel paper] The third aspect of the present invention provides an environmentally friendly high-insulation steel paper. The steel paper of the present invention uses environmentally friendly plant-derived raw materials and is environmentally friendly. At the same time, the steel paper of the present invention has a higher specific gravity and higher insulation strength than traditional steel paper, even more than twice that of traditional steel paper.
[0045] The thickness of the steel paper of the present invention is not limited and can be any desired thickness. For example, the thickness of the environmentally friendly high-insulation steel paper of the present invention is 0.02-5 mm, such as 0.5 mm, 0.6 mm, 0.8 mm, 1 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm, 2.0 mm, 2.5 mm, 3.0 mm, 3.5 mm, 4.0 mm, 4.5 mm, etc. It should be noted that the above thickness range is only an exemplary thickness, and those skilled in the art can produce steel paper beyond the above thickness range as needed.
[0046] The density of the steel paper of the present invention is not specific. Under the same conditions, the steel paper of the present invention has a higher density than the conventional steel paper. The exemplary density of the steel paper of the present invention is generally 1-2.5 kg / dm 3 , for example 1.2-2.4kg / dm 3 , 1.4-2.2kg / dm 3 1.5-2.0kg / dm 3 1.6-1.8kg / dm 3 wait.
[0047] The form of the steel paper of the present invention is not limited and can be processed into any desired form. Exemplary forms include plates, sheets, films, foils or flat strips.
[0048] Example 1 1. Raw material composition Raw material composition: Long fiber: absorbent cotton fiber, length 5-6mm, total fiber weight accounts for 95%; Short fiber: wood pulp fiber, with a length of 1-2mm, a Kappa number of 8, and a total fiber weight of 5%.
[0049] 2. Preprocessing After mixing in proportion, water is added and steamed for 1 hour to allow the fiber to fully absorb water and swell, while removing impurities. Next, the slurry enters the beater for beating treatment to further disperse and refine the fiber, with a beating degree of about 18°SR and a wet weight of about 10g.
[0050] 3. Paper The pre-treated slurry then enters the slurry mixing box for mixing to ensure uniform slurry. It is further transported to the slurry mixing box for dilution to adjust the slurry concentration and purified to further remove impurities.
[0051] The diluted and purified pulp is dehydrated through the paper machine mesh, and then further dehydrated in the pressing section. It is then sent to the drying section for drying to control the water content in the range of 4-8% to obtain steel paper base paper.
[0052] The obtained multi-layer steel paper base paper is simultaneously conveyed by a conveying roller into a potion (68% zinc chloride) for immersion for 1.5 minutes to fully swell and gelatinize the fibers, promote the connection between the fibers, and thus improve the strength and stability of the steel paper. Next, the soaked multi-layer base paper is heated at 30-40°C for 20-30 minutes to further penetrate the zinc chloride and gelatinize the fibers. Then, the multi-layer base paper is subjected to hot pressing to tightly bond the multi-layer base paper to form a semi-finished product.
[0053] 4. Post-processing The semi-finished product is sent to an aging furnace and aged at 20-40°C for about 50 minutes to improve the stability of the internal structure of the steel paper.
[0054] After aging, the steel paper is sequentially placed in multiple cleaning tanks with gradually decreasing concentrations and finally pure water for desalination treatment. The zinc chloride concentrations in the cleaning tanks are 60%, 30%, 15%, 8%, 4%, 2%, 1%, 0.5%, 0.05%, and 0. The desalination treatment time of each cleaning tank is controlled at 20-60 minutes, thereby making the surface of the steel paper smoother and more delicate. The product is dried.
[0055] Example 2 1. Raw material composition Raw material composition: Long fiber: absorbent cotton fiber, with a length of 5-6mm and a total fiber weight of 90%; Short fiber: wood pulp fiber, with a length of 1-2mm, a Kappa number of 8, and a total fiber weight of 10%.
[0056] 2. Preprocessing After mixing in proportion, water is added and steamed for 1 hour to allow the fiber to fully absorb water and swell, while removing impurities. Next, the slurry enters the beater for beating treatment to further disperse and refine the fiber, with a beating degree of about 15°SR and a wet weight of about 8g.
[0057] 3. Paper The pre-treated slurry then enters the slurry mixing box for mixing to ensure uniform slurry. It is further transported to the slurry mixing box for dilution to adjust the slurry concentration and purified to further remove impurities.
[0058] The diluted and purified pulp is dehydrated through the paper machine mesh, and then further dehydrated in the pressing section. It is then sent to the drying section for drying to control the water content in the range of 4-8% to obtain steel paper base paper.
[0059] The obtained multi-layer steel paper base paper is simultaneously conveyed by a conveying roller into a potion (68% zinc chloride) for immersion for 1.5 minutes to fully swell and gelatinize the fibers, promote the connection between the fibers, and thus improve the strength and stability of the steel paper. Next, the soaked multi-layer base paper is heated at 30-40°C for 20-30 minutes to further penetrate the zinc chloride and gelatinize the fibers. Then, the multi-layer base paper is subjected to hot pressing to tightly bond the multi-layer base paper to form a semi-finished product.
[0060] 4. Post-processing The semi-finished product is sent to an aging furnace and aged at 20-40°C for about 50 minutes to improve the stability of the internal structure of the steel paper.
[0061] After aging, the steel paper is sequentially placed in multiple cleaning tanks with gradually decreasing concentrations and finally pure water for desalination treatment. The zinc chloride concentrations in the cleaning tanks are 60%, 30%, 15%, 8%, 4%, 2%, 1%, 0.5%, 0.05%, and 0. The desalination treatment time of each cleaning tank is controlled at 20-60 minutes, thereby making the surface of the steel paper smoother and more delicate. The product is dried.
[0062] Example 3 1. Raw material composition Raw material composition: Long fiber: absorbent cotton fiber, with a length of 5-6mm and a total fiber weight of 92%; Short fiber: wood pulp fiber, with a length of 1-2mm, a Kappa number of 8, and a total fiber weight of 8%.
[0063] 2. Preprocessing After mixing in proportion, water is added and steamed for 1 hour to allow the fiber to fully absorb water and swell, while removing impurities. Next, the slurry enters the beater for beating treatment to further disperse and refine the fiber, with a beating degree of about 16°SR and a wet weight of about 9g.
[0064] 3. Paper The pre-treated slurry then enters the slurry mixing box for mixing to ensure uniform slurry. It is further transported to the slurry mixing box for dilution to adjust the slurry concentration and purified to further remove impurities.
[0065] The diluted and purified pulp is dehydrated through the paper machine mesh, and then further dehydrated in the pressing section. It is then sent to the drying section for drying to control the water content in the range of 4-8% to obtain steel paper base paper.
[0066] The obtained multi-layer steel paper base paper is simultaneously conveyed by a conveying roller into a potion (68% zinc chloride solution) for immersion for 1.5 minutes to fully swell and gelatinize the fibers, promote the connection between the fibers, and thus improve the strength and stability of the steel paper. Next, the soaked multi-layer base paper is heated at 30-40°C for 20-30 minutes to further penetrate the zinc chloride and gelatinize the fibers. Then, the multi-layer base paper is hot-pressed to tightly bond the multi-layer base paper to form a semi-finished product.
[0067] 4. Post-processing The semi-finished product is sent to an aging furnace and aged at 20-40°C for about 50 minutes to improve the stability of the internal structure of the steel paper.
[0068] After aging, the steel paper is sequentially placed in multiple cleaning tanks with gradually decreasing concentrations and finally pure water for desalination treatment. The zinc chloride concentrations in the cleaning tanks are 60%, 30%, 15%, 8%, 4%, 2%, 1%, 0.5%, 0.05%, and 0. The desalination treatment time of each cleaning tank is controlled at 20-60 minutes, thereby making the surface of the steel paper smoother and more delicate. The product is dried.
[0069] Example 4 1. Raw material composition Raw material composition: Long fiber: absorbent cotton fiber, length 8-10mm, total fiber weight accounts for 95%; Short fiber: wood pulp fiber, with a length of 1-2mm, a Kappa number of 10, and a total fiber weight of 5%.
[0070] 2. Preprocessing After mixing in proportion, water is added for cooking for 2 hours to allow the fiber to fully absorb water and swell, while removing impurities. Next, the slurry enters the beater for beating treatment to further disperse and refine the fiber, with a beating degree of about 17°SR and a wet weight of about 13g.
[0071] 3. Paper The pre-treated slurry then enters the slurry mixing box for mixing to ensure uniform slurry. It is further transported to the slurry mixing box for dilution to adjust the slurry concentration and purified to further remove impurities.
[0072] The diluted and purified pulp is dehydrated through the paper machine mesh, and then further dehydrated in the pressing section. It is then sent to the drying section for drying to control the water content in the range of 4-8% to obtain steel paper base paper.
[0073] The obtained multi-layer steel paper base paper is simultaneously conveyed by a conveying roller into a potion (68% zinc chloride solution) for immersion for 1.5 minutes to fully swell and gelatinize the fibers, promote the connection between the fibers, and thus improve the strength and stability of the steel paper. Next, the soaked multi-layer base paper is heated at 30-40°C for 20-30 minutes to further penetrate the zinc chloride and gelatinize the fibers. Then, the multi-layer base paper is hot-pressed to tightly bond the multi-layer base paper to form a semi-finished product.
[0074] 4. Post-processing The semi-finished product is sent to an aging furnace and aged at 20-40°C for about 50 minutes to improve the stability of the internal structure of the steel paper.
[0075] After aging, the steel paper is sequentially placed in multiple cleaning tanks with gradually decreasing concentrations and finally pure water for desalination treatment. The zinc chloride concentrations in the cleaning tanks are 60%, 30%, 15%, 8%, 4%, 2%, 1%, 0.5%, 0.05%, and 0. The desalination treatment time of each cleaning tank is controlled at 20-60 minutes, thereby making the surface of the steel paper smoother and more delicate. The product is dried.
[0076] Comparative Example 1 1. Raw material composition Raw material composition: Long fiber: absorbent cotton fiber, length 5-6mm, total fiber weight accounts for 80%; Short fiber: glass fiber cotton, its length is 1-2mm, and the total fiber weight accounts for 20%.
[0077] 2. Preprocessing After mixing in proportion, water is added and steamed for 1 hour to allow the fiber to fully absorb water and swell, while removing impurities. Next, the slurry enters the beater for beating treatment to further disperse and refine the fiber, with a beating degree of about 6°SR and a wet weight of about 10g.
[0078] 3. Paper The pre-treated slurry then enters the slurry mixing box for mixing to ensure uniform slurry. It is further transported to the slurry mixing box for dilution to adjust the slurry concentration and purified to further remove impurities.
[0079] The diluted and purified pulp is dehydrated through the paper machine mesh, and then further dehydrated in the pressing section. It is then sent to the drying section for drying to control the water content in the range of 4-8% to obtain steel paper base paper.
[0080] The obtained multi-layer steel paper base paper is simultaneously conveyed by a conveying roller into a potion (68% zinc chloride solution) for immersion for 1.5 minutes to fully swell and gelatinize the fibers, promote the connection between the fibers, and thus improve the strength and stability of the steel paper. Next, the soaked multi-layer base paper is heated at 30-40°C for 20-30 minutes to further penetrate the zinc chloride and gelatinize the fibers. Then, the multi-layer base paper is hot-pressed to tightly bond the multi-layer base paper to form a semi-finished product.
[0081] 4. Post-processing The semi-finished product is sent to an aging furnace and aged at 20-40°C for about 50 minutes to improve the stability of the internal structure of the steel paper.
[0082] After aging, the steel paper is sequentially placed in multiple cleaning tanks with gradually decreasing concentrations and finally pure water for desalination treatment. The zinc chloride concentrations in the cleaning tanks are 60%, 30%, 15%, 8%, 4%, 2%, 1%, 0.5%, 0.05%, and 0. The desalination treatment time of each cleaning tank is controlled at 20-60 minutes, thereby making the surface of the steel paper smoother and more delicate. The product is dried.
[0083] Comparative Example 2 1. Raw material composition Raw material composition: Long fiber: absorbent cotton fiber, length 5-6mm, total fiber weight accounts for 92%; Short fiber: wood pulp fiber, with a length of 1-2mm, a Kappa number of 25, and a total fiber weight of 8%.
[0084] 2. Preprocessing After mixing in proportion, water is added and steamed for 1 hour to allow the fiber to fully absorb water and swell, while removing impurities. Next, the slurry enters the beater for beating treatment to further disperse and refine the fiber, with a beating degree of about 10°SR and a wet weight of about 10g.
[0085] 3. Paper The pre-treated slurry then enters the slurry mixing box for mixing to ensure uniform slurry. It is further transported to the slurry mixing box for dilution to adjust the slurry concentration and purified to further remove impurities.
[0086] The diluted and purified pulp is dehydrated through the paper machine mesh, and then further dehydrated in the pressing section. It is then sent to the drying section for drying to control the water content in the range of 4-8% to obtain steel paper base paper.
[0087] The obtained multi-layer steel paper base paper is simultaneously conveyed by a conveying roller into a potion (68% zinc chloride solution) for immersion for 1.5 minutes to fully swell and gelatinize the fibers, promote the connection between the fibers, and thus improve the strength and stability of the steel paper. Next, the soaked multi-layer base paper is heated at 30-40°C for 20-30 minutes to further penetrate the zinc chloride and gelatinize the fibers. Then, the multi-layer base paper is hot-pressed to tightly bond the multi-layer base paper to form a semi-finished product.
[0088] 4. Post-processing The semi-finished product is sent to an aging furnace and aged at 20-40°C for about 50 minutes to improve the stability of the internal structure of the steel paper.
[0089] After aging, the steel paper is sequentially placed in multiple cleaning tanks with gradually decreasing concentrations and finally pure water for desalination treatment. The zinc chloride concentrations in the cleaning tanks are 60%, 30%, 15%, 8%, 4%, 2%, 1%, 0.5%, 0.05%, and 0. The desalination treatment time of each cleaning tank is controlled at 20-60 minutes, thereby making the surface of the steel paper smoother and more delicate. The product is dried.
[0090] Comparative Example 3 1. Raw material composition Raw material composition: Long fiber: cotton fiber, length 5-6mm, total fiber weight accounts for 95%; Short fiber: wood pulp fiber, with a length of 1-2mm, a Kappa number of 8, and a total fiber weight of 5%.
[0091] 2. Preprocessing After mixing in proportion, water is added and steamed for 1 hour to allow the fiber to fully absorb water and swell, while removing impurities. Next, the slurry enters the beater for beating treatment to further disperse and refine the fiber, with a beating degree of about 16°SR and a wet weight of about 9g.
[0092] 3. Paper The pre-treated slurry then enters the slurry mixing box for mixing to ensure uniform slurry. It is further transported to the slurry mixing box for dilution to adjust the slurry concentration and purified to further remove impurities.
[0093] The diluted and purified pulp is dehydrated through the paper machine mesh, and then further dehydrated in the pressing section. It is then sent to the drying section for drying to control the water content in the range of 4-8% to obtain steel paper base paper.
[0094] The obtained multi-layer steel paper base paper is simultaneously conveyed by a conveying roller into a potion (68% zinc chloride solution) for immersion for 1.5 minutes to fully swell and gelatinize the fibers, promote the connection between the fibers, and thus improve the strength and stability of the steel paper. Next, the soaked multi-layer base paper is heated at 30-40°C for 20-30 minutes to further penetrate the zinc chloride and gelatinize the fibers. Then, the multi-layer base paper is hot-pressed to tightly bond the multi-layer base paper to form a semi-finished product.
[0095] 4. Post-processing The semi-finished product is sent to an aging furnace and aged at 20-40°C for about 50 minutes to improve the stability of the internal structure of the steel paper.
[0096] After aging, the steel paper is sequentially placed in multiple cleaning tanks with gradually decreasing concentrations and finally pure water for desalination treatment. The zinc chloride concentrations in the cleaning tanks are 60%, 30%, 15%, 8%, 4%, 2%, 1%, 0.5%, 0.05%, and 0. The desalination treatment time of each cleaning tank is controlled at 20-60 minutes, thereby making the surface of the steel paper smoother and more delicate. The product is dried.
[0097] Comparative Example 4 1. Raw material composition Raw material composition: Cotton fiber, length 1-2mm, total fiber weight accounts for 95%; wood pulp fiber, length 1-2mm, Kappa number 8, total fiber weight accounts for 5%.
[0098] 2. Preprocessing After mixing in proportion, water is added and steamed for 1 hour to allow the fiber to fully absorb water and swell, while removing impurities. Next, the slurry enters the beater for beating treatment to further disperse and refine the fiber, with a beating degree of about 16°SR and a wet weight of about 8g.
[0099] 3. Paper The pre-treated slurry then enters the slurry mixing box for mixing to ensure uniform slurry. It is further transported to the slurry mixing box for dilution to adjust the slurry concentration and purified to further remove impurities.
[0100] The diluted and purified pulp is dehydrated through the paper machine mesh, and then further dehydrated in the pressing section. It is then sent to the drying section for drying to control the water content in the range of 4-8% to obtain steel paper base paper.
[0101] The obtained multi-layer steel paper base paper is simultaneously conveyed by a conveying roller into a potion (68% zinc chloride solution) for immersion for 1.5 minutes to fully swell and gelatinize the fibers, promote the connection between the fibers, and thus improve the strength and stability of the steel paper. Next, the soaked multi-layer base paper is heated at 30-40°C for 20-30 minutes to further penetrate the zinc chloride and gelatinize the fibers. Then, the multi-layer base paper is hot-pressed to tightly bond the multi-layer base paper to form a semi-finished product.
[0102] 4. Post-processing The semi-finished product is sent to an aging furnace and aged at 20-40°C for about 50 minutes to improve the stability of the internal structure of the steel paper.
[0103] After aging, the steel paper is sequentially placed in multiple cleaning tanks with gradually decreasing concentrations and finally pure water for desalination treatment. The zinc chloride concentrations in the cleaning tanks are 60%, 30%, 15%, 8%, 4%, 2%, 1%, 0.5%, 0.05%, and 0. The desalination treatment time of each cleaning tank is controlled at 20-60 minutes, thereby making the surface of the steel paper smoother and more delicate. The product is dried.
[0104] Comparative Example 5 1. Raw material composition Raw material composition: Absorbent cotton fiber, 1-2mm in length, accounts for 70% of the total fiber weight; brushed velvet (waste cotton produced by the brushing machine in the printing and dyeing factory), accounts for 30% of the total fiber weight.
[0105] 2. Preprocessing After mixing in proportion, water is added and boiled for 1 hour to allow the fiber to fully absorb water and swell while removing impurities. Next, the pulp enters the pulping machine for pulping.
[0106] 3. Paper The pre-treated slurry then enters the slurry mixing box for mixing to ensure uniform slurry. It is further transported to the slurry mixing box for dilution to adjust the slurry concentration and purified to further remove impurities.
[0107] The diluted and purified pulp is dehydrated through the paper machine mesh, and then further dehydrated in the pressing section. It is then sent to the drying section for drying to control the water content in the range of 4-8% to obtain steel paper base paper.
[0108] The obtained multi-layer steel paper base paper is simultaneously conveyed by a conveying roller into a potion (68% zinc chloride) for immersion for 1.5 minutes to fully swell and gelatinize the fibers, promote the connection between the fibers, and thus improve the strength and stability of the steel paper. Next, the soaked multi-layer base paper is heated at 30-40°C for 20-30 minutes to further penetrate the zinc chloride and gelatinize the fibers. Then, the multi-layer base paper is subjected to hot pressing to tightly bond the multi-layer base paper to form a semi-finished product.
[0109] 4. Post-processing The semi-finished product is sent to an aging furnace and aged at 20-40°C for about 50 minutes to improve the stability of the internal structure of the steel paper.
[0110] After aging, the steel paper is sequentially placed in multiple cleaning tanks with gradually decreasing concentrations and finally pure water for desalination treatment. The zinc chloride concentrations in the cleaning tanks are 60%, 30%, 15%, 8%, 4%, 2%, 1%, 0.5%, 0.05%, and 0. The desalination treatment time of each cleaning tank is controlled at 20-60 minutes, thereby making the surface of the steel paper smoother and more delicate. The product is dried.
[0111] Test Case 1. Electrical strength test of insulation materials According to GB / T 1408.1-2016 "Electrical strength test methods for insulating materials Part 1: Tests at power frequency", the dielectric strength of steel paper under power frequency (50Hz) voltage is measured. The specific steps are as follows: Sample preparation: The thickness of the sample is 3 mm, and the two surfaces of the sample in contact with the electrode should be parallel and as flat and smooth as possible.
[0112] Electrode preparation: Stainless steel rods are usually used as electrodes with a diameter of 6 ± 0.1 mm and a rounded edge radius of 1 ± 0.2 mm. The electrodes should be installed vertically in the electrode holder so that one electrode is above the other. The gap between the protected electrode and the guarding electrode is twice the thickness of the sample. The diameter of the protected electrode is 10 times the thickness of the sample.
[0113] Test conditions: The test is carried out under environmental conditions of 23±2℃ and 50±5%RH. The specimens are conditioned under these conditions for at least 24 hours. The thickness of the specimens is measured to 0.1mm.
[0114] Test process: The sample is placed between two electrodes in a stretched state. The voltage applied to the sample starts from zero and gradually increases at a uniform rate (such as 500V / s) until breakdown occurs.
[0115] The electrical strength is the ratio of the breakdown voltage to the electrode spacing, and the median value of three samples is taken as the final result.
[0116] Data recording and analysis: The breakdown voltage and electrical strength of each specimen were recorded.
[0117] 2. Tensile Strength Measurement Experiment According to GB / T 12914-2018 "Paper and paperboard - Determination of tensile strength - Constant tension method (20mm / min)", use a tensile tester to stretch a sample of specified size to break at a constant tensile speed, record its tensile force and elongation at the same time. Continuously record the tensile force and elongation, and determine the elongation at break, tensile energy absorption and elastic modulus. The specific steps are as follows: 1. Adjustment and calibration of the tester The tester should be calibrated according to the manufacturer's instructions so that the elongation at break is accurate to ±0.1 mm. The clamp position should be set correctly so that the test distance is 20 mm ± 0.5 mm. The test speed should be adjusted. The clamping pressure should be adjusted so that the specimen has neither slippage nor damage.
[0118] 2. Sample preparation The tensile index is determined according to GB / T451.2. If the elastic modulus needs to be determined, the thickness of the sample is determined according to GB / T451.2. From the non-destructive sample, cut a sample with a width of 15mm±0.1mm and hold it between the two ends. Avoid touching the test area of the sample with bare hands. There should be no watermarks, creases and wrinkles in the test area. Ensure that the sample is representative of the sample being tested. The two long sides of the sample should be straight, and its parallelism should not exceed ±0.1 mm throughout the clamping length. The incision should be neat and undamaged. Cut a sufficient number of samples to perform 10 tests in each required direction (longitudinal or transverse).
[0119] 3. Test steps Make sure the tester has been calibrated as above. Place the specimen in the grips and gently straighten the specimen to eliminate any visible slack. Avoid touching the test area between the grips with your fingers. Grip the specimen firmly and test. Perform 10 tests in each required direction (longitudinal or transverse).
[0120] 4. Technical parameters Measuring range: 50N, 100N, 200N, etc. optional Resolution: 0.01N Accuracy: ±1% Test speed: (5-500) mm / min Return speed: 300 mm / min adjustable Test stroke: 680mm adjustable Dimensions: 400×500×1200 mm Mass: Approx. 68kg.
[0121] 3. Water absorption According to GB / T 461.3-2005 "Paper and paperboard - Determination of water absorption (immersion method)", the specific steps are as follows: 1. Sample preparation According to GB / T 450. Sample treatment is carried out according to GB / T 10739. The temperature and humidity treatment is carried out under this atmospheric condition. The sample is cut into 10 square samples of 100mm×100mm.
[0122] 2. Test steps Place the treated sample in a pre-weighed clean container and weigh it on a balance. Take the sample out of the container and insert it vertically into a reagent tank filled with distilled water. The upper edge of the sample should be 25mm±3mm below the water surface, and avoid contact between the sample and the bottom of the tank or between samples. The immersion time is 30min±60s.
[0123] If it is uncertain whether the immersion time can fully saturate the specimen, another specimen shall be used to determine the flooding time first, and then the test shall be carried out according to the test procedure, and the flooding time in distilled water again shall be at least half of the initial time. If the selected flooding time can fully saturate the specimen, the next shorter time shall be used (unless otherwise specified).
[0124] 3. After the sample has been immersed in distilled water for the specified time, use tweezers to vertically clamp one corner of the sample and take it out of the distilled water. Clamp the sample for 2 minutes to allow the distilled water to drip. Put the sample back into the original container and weigh it on a balance to an accuracy of 0.01g.
[0125] 4. Result calculation The relative water absorption is calculated according to the following formula, and the result should be expressed as the average value of 10 measurements, accurate to 0.1%.
[0126] R = (m2-m1) / m1×100%; in: R--Relative water absorption, %; m1--The mass of the sample before water absorption, in g; m2--The mass of the sample after absorbing water, in g.
[0127] The test results are shown in Table 1 below.
[0128] Table 1 Although the present invention has been described with reference to exemplary embodiments, it should be understood that the present invention is not limited to the disclosed exemplary embodiments. Various adjustments or changes may be made to the exemplary embodiments of the present specification without departing from the scope or spirit of the present invention. The scope of the claims should be based on the broadest interpretation to cover all modifications and equivalent structures and functions.
Claims
1. An environmentally friendly high-insulation steel pulp composition, characterized in that: The slurry composition comprises 90-95 parts by weight of long fibers and 5-10 parts by weight of short fibers, wherein the long fibers are absorbent cotton fibers with a length of 2-25 mm, the short fibers are wood pulp fibers with a length of 1-2 mm, and the long fibers and the short fibers are respectively hydrophilic fibers, and the slurry composition does not contain inorganic fibers.
2. The environmentally friendly high-insulation steel pulp composition according to claim 1, characterized in that: The length of the long fibers is 3-10 times the length of the short fibers.
3. The environmentally friendly high-insulation steel pulp composition according to claim 1, characterized in that: The kappa number of the wood pulp fiber is 5-20.
4. The environmentally friendly high-insulation steel pulp composition according to claim 1, characterized in that: The inorganic fibers include glass fibers.
5. A method for preparing environmentally friendly high-insulation steel paper, characterized in that: The following steps are involved: (1) The pulp composition according to any one of claims 1 to 4 is passed through a pulping machine for pulping, and then passed through a stock preparation box for mixing, and further subjected to dilution and / or purification treatment, and subjected to dehydration treatment in a papermaking machine to form a wet paper web, and the water content is controlled within the range of 4-8% by pressing and drying to obtain steel paper base paper; (2) soaking the multi-layer steel paper in a solution for 1-10 minutes, wherein the solution is a 50-88 wt % zinc chloride solution; (3) heating and pressurizing the soaked multi-layer steel paper base paper to form a semi-finished product; (4) The product is aged at 20-40°C, desalted and dried to obtain environmentally friendly high-insulation steel paper.
6. The method for preparing the environmentally friendly high-insulation steel paper according to claim 5, characterized in that: Before the step (1), the method further comprises the step of adjusting the kappa number of the short fibers to 5-20.
7. The method for preparing the environmentally friendly high-insulation steel paper according to claim 5, characterized in that: In the step (1), the beating degree is 15-25°SR and the wet weight is 8-18g.
8. The method for preparing the environmentally friendly high-insulation steel paper according to claim 5, characterized in that: After the step (4), the method further comprises the step of shaping by a calender.
9. An environmentally friendly high-insulation steel paper, characterized in that: The slurry is prepared using the slurry composition described in any one of claims 1 to 4, or is prepared by the method described in any one of claims 5 to 8.
10. The environmentally friendly high-insulation steel paper according to claim 9, characterized in that: Its thickness is 0.02-5mm and its density is 1-2.5kg / dm 3 .
Citation Information
Patent Citations
Flame-retardant insulation vulcanized fiber board and manufacturing technique thereof
CN103088701A
Vulcanized paper raw paper and manufacturing process thereof
CN103132365A
Abrasive steel paperboard and manufacturing process thereof
CN103147356A
Environment-friendly vulcanized fiber paper and production process thereof
CN107227658A
Heat-resistant hard paper and preparing method thereof
CN109355975A