Method for obtaining in-situ interface type-2 fracture toughness of three-dimensional woven composite material

By cutting small-sized off-axis compression test pieces on a three-dimensional woven composite material plate and combining test and simulation, the problem of difficulty in measuring the interface of the three-dimensional woven composite material in the prior art is solved, and a more accurate material is achieved Performance evaluation.

CN118980571AActive Publication Date: 2024-11-19HARBIN INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411063948.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The prior art is difficult to effectively test the interfacial mechanical properties of three-dimensional woven composite materials, especially the type 2 fracture toughness parameters, which leads to high measurement results or the inability to extract independent interface structures, affecting material performance evaluation and simulation research.

Method used

By designing small-sized off-axis compression test pieces, prefabricated cracks are cut on three-dimensional woven composite material plates, and combining tests and simulations, a high-fidelity finite element model is established, and the crack propagation process is simulated using virtual crack closure technology to obtain the interface Type 2 fracture toughness.

Benefits of technology

Accurate type 2 fracture toughness testing of the interface of three-dimensional woven composite materials is realized, which improves the accuracy and efficiency of the test and ensures reliable evaluation of the interface mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980571A_ABST
    Figure CN118980571A_ABST
Patent Text Reader

Abstract

The invention discloses a method for obtaining in-situ interface type-2 fracture toughness of a three-dimensional woven composite material, an internal yarn woven structure of the three-dimensional woven composite material comprises warp yarns and weft yarns, space interlocking exists between the two kinds of yarns, the fluctuation direction of the warp yarns is the first direction of a local coordinate system of a composite material plate, the fluctuation direction of the weft yarns is the second direction of the local coordinate system of the composite material plate, and the fluctuation direction of the warp yarns is the first direction of the local coordinate system of the composite material plate. The thickness direction is three, and the method comprises the following steps: step 1, designing a small-size off-axis compression test piece, and cutting a prefabricated crack at a specified position; 2, establishing a high-fidelity finite element model according to the test piece structure; according to the cutting position and size design of the test piece, an independent and simple interface structure is formed in the test piece, and testing of the interface mechanical property is facilitated. The position and length of the notch at the tail end of the test piece can ensure stable expansion of the type-II crack along the interface of the test piece. The test piece is small in size and simple in structure, the establishment of a high-fidelity full-size finite element model is facilitated, and the modeling efficiency and precision are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of composite material mechanical property testing, and relates to a method for testing the interface mechanical properties between components (fiber bundle / fiber bundle or fiber bundle / matrix) of a three-dimensional woven composite material, and specifically to a method for obtaining the mode II fracture toughness of an in-situ interface of a three-dimensional woven composite material by combining experiments with simulations. Background Art

[0002] In recent years, fiber-reinforced composites have been widely used in various fields such as aerospace, shipbuilding, automobiles, and sports due to their excellent mechanical properties such as specific modulus and specific strength. Compared with traditional laminated composites, three-dimensional woven composites have better anti-delamination and impact resistance and have broad application prospects. The spatial structure of the three-dimensional woven composite preform is complex and diverse, which also makes the material as a whole present diverse mechanical properties. A large number of experimental studies have shown that in three-dimensional woven composites, interfacial debonding between component materials is the core failure mode, which significantly affects the allowable load and damage mechanism of the material. Therefore, how to obtain the interfacial mechanical properties of three-dimensional woven composites is of great significance to the evaluation of the overall performance of the material.

[0003] Due to the novelty of three-dimensional woven composites, the test methods suitable for the interlayer performance test of traditional laminated composites are no longer suitable for three-dimensional woven composites. Studies have shown that the traditional type II fracture toughness test method will cause the waving yarn of three-dimensional woven composites to break, resulting in a measurement result that is more than ten times higher. The interface structure of three-dimensional woven composites is very complex and small in size, which brings great difficulties to the design of test pieces. Conventional-sized specimens cannot extract independent interface structures, so they are not suitable for interface mechanical properties testing. Using small-sized specimens can extract independent interface structures, but the location selection of the specimens and the processing accuracy of the specimens need to be carefully studied. These works have brought great difficulties to the interface mechanical properties testing, so no research has yet proposed a method for obtaining the type II fracture toughness of the interface of three-dimensional woven composites. However, this parameter is of great significance to the performance evaluation of materials and the simulation research of three-dimensional woven composites. Therefore, it is very necessary to carry out research on the type II fracture toughness of the interface of three-dimensional woven composites. Summary of the invention

[0004] In view of the fact that the method field of obtaining the mode II fracture toughness of the interface of three-dimensional woven composite materials is still blank, the present invention provides a method for obtaining the in-situ mode II fracture toughness of the interface of three-dimensional woven composite materials in order to fill the blank in this research field. In this method, in-situ means in-situ material collection, directly processing the specimen on the composite material plate, and the interface refers to the component materials, that is, the fiber bundle / fiber bundle interface or the fiber bundle / matrix interface.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] A method for obtaining in-situ interface mode II fracture toughness of a three-dimensional woven composite material, wherein the internal yarn weaving structure of the three-dimensional woven composite material includes warp yarns and weft yarns, there is spatial interlocking between the two yarns, the warp yarn fluctuation direction is the 1 direction of the local coordinate system of the composite material plate, the weft yarn fluctuation direction is the 2 direction of the local coordinate system of the composite material plate, and the thickness direction is the 3 direction of the local coordinate system of the composite material plate, comprising the following steps:

[0007] Step 1: Design a small-sized eccentric compression test piece and cut a prefabricated crack at a specified position. The cutting position of the test piece is determined according to the wave structure of the fiber bundle in the material. The specific steps are as follows:

[0008] Step 1-1: In a three-dimensional woven composite material plate, find a weft yarn section in a plane formed by direction 1 and direction 3, and cut a thin plate that does not exceed the width of the weft yarn section according to the position of the weft yarn section;

[0009] Step 1-2: After removing the thin plate, cut an eccentric compression specimen on the thin plate, make a prefabricated crack at one end of the specimen, and the prefabricated crack must be cut along the material cross section;

[0010] Step 2: Establish a high-fidelity finite element model based on the specimen structure. The specific steps are as follows:

[0011] Step 2-1: Take a photo of the specimen surface to obtain geometric information of the specimen surface;

[0012] Step 2-2: Based on the geometric information of the specimen surface, a geometric model for restoring the specimen structure is established;

[0013] Step 2-3: Mesh the geometric model and simulate the crack propagation process using virtual crack closure technology in the interface area connected by the prefabricated cracks;

[0014] Step 2-4: Add material properties to the fiber bundle and matrix respectively, and correct the main material directions of the warp and weft yarns in different directions to ensure the accuracy of the finite element model;

[0015] Step 3: Based on the crack initiation load in the test, compare it with the crack initiation load in the finite element model to obtain the mode II fracture toughness of the specimen interface. The specific steps are as follows:

[0016] Step 3-1: Obtain the strain and displacement information near the prefabricated crack tip of the specimen;

[0017] Step 3-2: Assemble the compression fixture and the specimen, and place the assembled compression fixture and the specimen as a whole on the compression disc of the quasi-static testing machine;

[0018] Step 3-3: After preloading, use the displacement control testing machine to start the compression test until obvious crack propagation is observed on the surface of the specimen, and use the quasi-static testing machine to output information such as load, displacement and time during the test;

[0019] Step 3-4: Observe the crack propagation on the surface of the specimen and record the time of crack initiation;

[0020] Step 3-5: Find the compression load corresponding to the crack initiation based on the recorded crack initiation time and the load-time information output by the quasi-static testing machine;

[0021] Step 3-6: Apply boundary conditions consistent with those of the test piece to the finite element model, and determine the accuracy of the finite element model by comparing the displacement field on the surface of the test piece with the displacement field of the finite element model;

[0022] Step 3-7: After verifying the accuracy of the finite element model, adjust the mode II fracture toughness value of the interface in the virtual crack closure technique and compare the crack initiation load in the finite element model with the crack initiation load observed in the experiment;

[0023] Step 3-8: When the result of the finite element model is close to the test result (within 1% deviation), the interface mode II fracture toughness input into the finite element model is the mode II fracture toughness of the interface of the three-dimensional woven composite material.

[0024] Compared with the prior art, the present invention has the following advantages:

[0025] 1. The cutting position and size design of the test piece proposed in the present invention enable the test piece to have an independent and simple interface structure, which is beneficial to the testing of the mechanical properties of the interface.

[0026] 2. The position and length of the notch at the end of the specimen can ensure the stable extension of the mode II crack along the specimen interface.

[0027] 3. The specimen is small in size and simple in structure, which is conducive to the establishment of a high-fidelity full-size finite element model and improves modeling efficiency and accuracy.

[0028] 4. The combination of experiment and simulation is conducive to obtaining more accurate interface mode II fracture toughness. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a typical internal yarn braiding structure of a three-dimensional woven composite material;

[0030] Figure 2 is a typical specimen cutting position;

[0031] Figure 3 This is an example of the assembly of the specimen and the fixture;

[0032] Figure 4 To obtain the process of interface mode II fracture toughness;

[0033] Figure 5 It is a comparative analysis of typical test results and finite element models;

[0034] Figure 6 This is a typical crack extension phenomenon. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described below in conjunction with the accompanying drawings, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.

[0036] The present invention provides a method for obtaining the in-situ interface mode II fracture toughness of a three-dimensional woven composite material. The research object of the method is a three-dimensional woven composite material, such as Figure 1 As shown in the figure, the internal yarn weaving structure of the three-dimensional woven composite material includes warp yarn and weft yarn, and there is spatial interlocking between the two yarns. The warp yarn fluctuates significantly, and the weft yarn is relatively straight. The warp yarn fluctuates in the 1 direction of the local coordinate system of the composite plate, the weft yarn fluctuates in the 2 direction, and the thickness direction is the 3 direction.

[0037] Figure 2 This is a typical eccentric compression specimen cutting position. In the three-dimensional machined material plate, find the weft section in the 1-3 plane, and cut a thin plate that does not exceed the width of the weft section according to the weft section position. After removing the thin plate, cut the eccentric compression specimen on the thin plate, and make a prefabricated crack at one end of the specimen. The prefabricated crack must be cut along the material section.

[0038] Figure 3 This is an example of the assembly of the specimen and the compression fixture. The compression fixture includes a fixture body, a cover plate and a cylindrical guide rail. The fixture body consists of an upper fixture and a lower fixture. The upper fixture and the lower fixture are connected by two cylindrical guide rails, wherein: through holes are provided on the opposite surfaces of the upper fixture and the lower fixture, and the two ends of the cylindrical guide rail are located in the through holes. The through holes and the surfaces of the cylindrical guide rails should be tightly matched and have low friction to ensure accurate test results; the surface of the compression fixture in contact with the specimen needs to be polished. The fixture body and the cover plate are connected by bolts to press the specimen, limit the out-of-plane displacement of the specimen, and prevent the specimen from buckling. The parallelism between the parallel surfaces of the upper fixture and the lower fixture must be strictly guaranteed.

[0039] Figure 4 The process for obtaining the interface mode II fracture toughness specifically includes the following steps:

[0040] Step 1: In the three-dimensional woven composite material plate, an eccentric compression specimen is cut along the plane formed by direction 1 and direction 3.

[0041] Step 2: Take a photo of the specimen surface to obtain the geometric information of the specimen.

[0042] Step 3: Spray the speckle on the surface of the specimen, and use digital image correlation technology (or crack meter) to obtain the strain and displacement information near the prefabricated crack tip. Assemble the fixture and the specimen, and place the assembled fixture and specimen on the compression disc of the testing machine. After preloading, start the compression test using the displacement control testing machine until obvious crack extension is observed on the surface of the specimen. Use the testing machine to output information such as load, displacement, and time during the test.

[0043] Step 4: Observe the crack propagation on the specimen surface. The reasonable crack propagation position is as follows: Figure 6 As shown. The crack must propagate along the interface along the tip of the prefabricated crack. The time of crack initiation is recorded by digital image correlation analysis (or by observing the results of the crack meter). If other damage modes or cracks at other locations propagate before the crack tip of the prefabricated crack during the test, this test method is not applicable to the three-dimensional woven composite material of this material system.

[0044] Step 5: Based on the recorded crack initiation time and the load-time information output by the testing machine, find the compression load corresponding to the crack initiation.

[0045] Step 6: According to the geometric information of the specimen surface, a finite element model is established to restore the specimen structure. The geometric model is meshed, and the virtual crack closure technology is used to simulate the crack propagation process in the interface area connected to the prefabricated cracks. Material properties are added to the fiber bundle and matrix respectively, and the main material directions of the warp and weft yarns in different directions are corrected respectively.

[0046] Step 7: Apply boundary conditions consistent with those of the test piece to the finite element model. First, the accuracy of the finite element model is determined by comparing the displacement field of the specimen surface with the displacement field of the finite element model. After verifying the accuracy of the model, adjust the mode II fracture toughness value of the interface in the virtual crack closure technology and compare the crack initiation load in the finite element model with the crack initiation load observed in the experiment.

[0047] Step 8: Figure 5 This is a typical comparison between the test results and the finite element model calculation results. When the input fracture toughness value of the finite element model is 0.5N / mm, the crack initiation load in the finite element model is consistent with the test results. At this time, the interface mode II fracture toughness input in the finite element model is the mode II fracture toughness of the interface of the three-dimensional woven composite material.

Claims

1. A method for obtaining in-situ interface mode II fracture toughness of three-dimensional woven composite materials, Features The internal yarn weaving structure of the three-dimensional woven composite material includes warp yarns and weft yarns, and there is spatial interlocking between the two yarns. The warp yarn fluctuation direction is the 1 direction of the local coordinate system of the composite material plate, the weft yarn fluctuation direction is the 2 direction of the local coordinate system of the composite material plate, and the thickness direction is the 3 direction of the local coordinate system of the composite material plate, including the following steps: Step 1: Design a small-sized eccentric compression test piece and cut a prefabricated crack at the specified position. The specific steps are as follows: Step 1-1: In a three-dimensional woven composite material plate, find a weft yarn section in a plane formed by directions 1 and 3, and cut a thin plate that does not exceed the width of the weft yarn section according to the position of the weft yarn section; Step 1-2: After removing the thin plate, cut an eccentric compression specimen on the thin plate, make a prefabricated crack at one end of the specimen, and the prefabricated crack must be cut along the material cross section; Step 2: Establish a high-fidelity finite element model based on the specimen structure. The specific steps are as follows: Step 2-1: Take a photo of the specimen surface to obtain geometric information of the specimen surface; Step 2-2: Based on the geometric information of the specimen surface, a geometric model for restoring the specimen structure is established; Step 2-3: Mesh the geometric model and simulate the crack propagation process using virtual crack closure technology in the interface area connected by the prefabricated cracks; Step 2-4: Add material properties to the fiber bundle and matrix respectively, and correct the main material directions of the warp and weft yarns in different directions to ensure the accuracy of the finite element model; Step 3: Based on the crack initiation load in the test, compare it with the crack initiation load in the finite element model to obtain the mode II fracture toughness of the specimen interface. The specific steps are as follows: Step 3-1: Obtain the strain and displacement information near the prefabricated crack tip of the specimen; Step 3-2: Assemble the compression fixture and the specimen, and place the assembled compression fixture and the specimen as a whole on the compression disc of the quasi-static testing machine; Step 3-3: After preloading, use the displacement control testing machine to start the compression test until obvious crack propagation is observed on the surface of the specimen, and use the quasi-static testing machine to output information such as load, displacement and time during the test; Step 3-4: Observe the crack propagation on the surface of the specimen and record the time of crack initiation; Step 3-5: Find the compression load corresponding to the crack initiation based on the recorded crack initiation time and the load-time information output by the quasi-static testing machine; Step 3-6: Apply boundary conditions consistent with those of the test piece to the finite element model, and determine the accuracy of the finite element model by comparing the displacement field on the surface of the test piece with the displacement field of the finite element model; Step 3-7: After verifying the accuracy of the finite element model, adjust the mode II fracture toughness value of the interface in the virtual crack closure technique and compare the crack initiation load in the finite element model with the crack initiation load observed in the experiment; Step 3-8: When the result of the finite element model is close to the test result, the interface mode II fracture toughness input into the finite element model is the mode II fracture toughness of the interface of the three-dimensional woven composite material.

2. The method for obtaining in-situ interface mode II fracture toughness of a three-dimensional woven composite material according to claim 1, Features In the step 3-1, the speckle pattern is sprayed on the surface of the specimen, and the strain and displacement information near the prefabricated crack tip is obtained using digital image correlation technology or a crack meter.

3. The method for obtaining in-situ interface mode II fracture toughness of a three-dimensional woven composite material according to claim 1, Features In step 3-2, the compression clamp includes a clamp body, a cover plate and a cylindrical guide rail. The clamp body consists of an upper clamp and a lower clamp. The upper clamp and the lower clamp are connected by two cylindrical guide rails, and the clamp body and the cover plate are connected by bolts.

4. The method for obtaining in-situ interface mode II fracture toughness of a three-dimensional woven composite material according to claim 1, Features In the steps 3-8, the deviation between the result of the finite element model and the test result is within 1%.

Citation Information

Patent Citations

  • Method for obtaining interfacial strength of three-dimensional woven composite material

    CN112595593A

  • Method for testing II-type interlayer cracks of arc-shaped composite material

    CN115901456A

  • Method for determining interlayer fracture toughness and bridging stress of composite material in over-notch bending test

    CN118150332A

  • Method and device for measuring fracture toughness of fiber-reinforced composite material

    JP1996101105A