P-type thin film transistor and preparation method thereof
By using alternately arranged metal layers and semiconductor oxide layers in P-type thin film transistors to form a multi-layer channel layer, and using magnetron sputtering technology to optimize the conductance path, the existing P-type thin film transistors have low mobility and low mobility and The problem of poor stability significantly improves electrical performance and switching ratio.
Patent Information
- Application Number
- CN202411079588.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
AI Technical Summary
The low mobility and poor stability of existing P-type thin film transistors limit the application and development of transparent oxide electrons.
The channel layer with a multi-layer structure is formed by alternately arranged metal layers and semiconductor oxide layers. Deposition is optimized through magnetron sputtering technology, and the possibility of interface scattering and carrier recombination is reduced.
The mobility and electrical performance of P-type thin film transistors are improved, the switching ratio is improved, and the stability and performance of the device are improved.
Smart Images

Figure CN118983343A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor optoelectronics, and in particular to a P-type thin film transistor and a preparation method thereof. Background Art
[0002] Transparent oxide thin film transistors have been widely studied. Due to their main characteristics of visible light transparency and current regulation, they are mainly used in displays, flexible wearable devices and other electronic circuit fields. Since N-type oxide semiconductors have the characteristics of high light transmittance and high electron mobility, some current research focuses on N-type oxide semiconductors, while both N-type and P-type transistors are required to form complementary circuits. However, P-type thin film transistors still face disadvantages such as low mobility and poor stability. The performance of P-type thin film transistors such as Cu2O, SnO, Ag2O, WO3, and NiO reported so far is much lower than that of N-type thin film transistors. The lack of high-performance P-type oxide semiconductors and P-type thin film transistors severely limits the application and development of oxide transparent electronics. Summary of the invention
[0003] The object of the present invention is to provide a P-type thin film transistor and a method for manufacturing the same, so as to improve the technical problem of poor electrical performance of the P-type thin film transistor in the prior art.
[0004] In order to solve the above technical problems, the present invention first provides a P-type thin film transistor, comprising a substrate, a gate dielectric layer, a channel layer, a source electrode and a drain electrode, wherein the gate dielectric layer is formed on the surface of the substrate, and the channel layer is formed on the surface of the gate dielectric layer; the source electrode and the drain electrode are both formed on the surface of the channel layer and contact with a portion of the gate dielectric layer, and there is a gap between the source electrode and the drain electrode; The channel layer includes at least one metal layer and at least two semiconductor oxide layers which are alternately arranged, each metal layer is inserted between two adjacent semiconductor oxide layers; and at least one semiconductor oxide layer is in contact with the gate dielectric layer.
[0005] Preferably, the material of the semiconductor oxide layer is any one of Ga2O3, In2O3 and TiO2, and the material of the metal layer is at least one of Zn and Au.
[0006] Preferably, the thickness of the semiconductor oxide layer is a, and the thickness of the metal layer is b, wherein the relationship between a and b is as follows: a≥10b; 0≤b≤2nm.
[0007] Preferably, the number of semiconductor oxide layers is c, and the number of metal layers is d, wherein the relationship between c and d is as follows: c=d+1, 1≤d≤50, and c and d are both positive integers.
[0008] Preferably, the base is made of silicon substrate material, and the material of the gate dielectric layer is at least one of silicon nitride and silicon dioxide.
[0009] Preferably, the material of the source electrode and the drain electrode is at least one of molybdenum, titanium, silver, aluminum and copper.
[0010] Accordingly, the present invention further provides a method for preparing a P-type thin film transistor as described above, the method comprising: S10, forming a gate dielectric layer on the substrate; S20, alternately depositing semiconductor oxide layers and metal layers on the gate dielectric layer, with each metal layer inserted between two adjacent semiconductor oxide layers, to finally obtain a channel layer; S30, forming a source electrode and a drain electrode spaced apart from each other on the channel layer, wherein both the source electrode and the drain electrode are in contact with a portion of the gate dielectric layer.
[0011] Preferably, in step S20, a physical vapor deposition method is used to alternately deposit semiconductor oxide layers and metal layers on the gate dielectric layer, and the physical vapor deposition method uses any one or any combination of electron beam evaporation, molecular beam epitaxial film deposition, DC reactive magnetron sputtering and radio frequency magnetron sputtering methods.
[0012] Preferably, in step S20, the thickness and film formation time of the semiconductor oxide layer or the metal layer are controlled by controlling at least one parameter of the substrate temperature, sputtering time, reaction gas content and sputtering power.
[0013] Preferably, in step S20, the material of the semiconductor oxide layer is any one of Ga2O3, In2O3 and TiO2, and the material of the metal layer is at least one of Zn and Au.
[0014] The beneficial effects of the present invention are as follows: Different from the prior art, the present invention provides a P-type thin film transistor and a preparation method thereof, wherein the P-type thin film transistor comprises a substrate, a gate dielectric layer, a channel layer, a source electrode and a drain electrode, wherein the gate dielectric layer is formed on the surface of the substrate, and the channel layer is formed on the surface of the gate dielectric layer; the source electrode and the drain electrode are both formed on the surface of the channel layer and contact with part of the gate dielectric layer, and there is a gap between the source electrode and the drain electrode, wherein the channel layer comprises at least one metal layer and at least two semiconductor oxide layers arranged alternately, each metal layer is inserted between two adjacent semiconductor oxide layers; and at least one semiconductor oxide layer is in contact with the gate dielectric layer. The present invention arranges the channel layer in the P-type thin film transistor into a multilayer structure formed alternately of semiconductor oxide layers and metal layers, and by inserting a metal layer between two adjacent semiconductor oxide layers, the conductance path can be optimized, the influence of interface scattering on carrier mobility can be reduced, the possibility of carrier recombination can be reduced to improve mobility, and thus the switching ratio of the P-type thin film transistor can be improved, and finally the electrical performance of the P-type thin film transistor can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 is a schematic diagram of the cross-sectional structure of a P-type thin film transistor provided in an embodiment of the present invention; Figure 2 It is a schematic diagram of the cross-sectional structure between the channel layer and the gate dielectric layer in the P-type thin film transistor provided by an embodiment of the present invention; Figure 3 is a flow chart of a method for preparing a P-type thin film transistor provided by an embodiment of the present invention; Figure 4 is a transfer curve diagram of a P-type thin film transistor provided in Example 1 of the present invention; In the figure, 100 is a P-type thin film transistor 100; 11 is a substrate; 11 is a gate dielectric layer; 13 is a channel layer; 131 is a semiconductor oxide layer; 132 is a metal layer; 14 is a source electrode; and 15 is a drain electrode. DETAILED DESCRIPTION
[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] In view of the problem that the electrical performance of the currently prepared P-type thin film transistor 100 is poor, the present invention adopts magnetron sputtering to alternately deposit oxide and metal to form the channel layer 13 of the P-type thin film transistor 100, so that the P-type thin film transistor 100 with excellent performance can be prepared, and its on / off ratio can be as high as 104 ~10 6 .
[0018] See also Figure 1 to Figure 2 , Figure 1 is a schematic cross-sectional structure diagram of a P-type thin film transistor 100 provided in an embodiment of the present invention, Figure 2 1 is a schematic diagram of a cross-sectional structure between a channel layer 13 and a gate dielectric layer 12 in a P-type thin film transistor 100 provided in an embodiment of the present invention; wherein the P-type thin film transistor 100 comprises a substrate 11, a gate dielectric layer 12, a channel layer 13, a source electrode 14 and a drain electrode 15, the gate dielectric layer 12 is formed on a surface of the substrate 11, and the channel layer 13 is formed on a surface of the gate dielectric layer 12; the source electrode 14 and the drain electrode 15 are both formed on a surface of the channel layer 13 and contact a portion of the gate dielectric layer 12, and there is a gap between the source electrode 14 and the drain electrode 15; The channel layer 13 includes at least one metal layer 132 and at least two semiconductor oxide layers 131 that are alternately arranged, and each metal layer 132 is inserted between two adjacent semiconductor oxide layers 131 ; at least one semiconductor oxide layer 131 is in contact with the gate dielectric layer 12 .
[0019] In this embodiment, the substrate 11 is a silicon substrate material or a glass substrate, and the material of the gate dielectric layer 12 is at least one of silicon nitride and silicon dioxide; wherein, when the substrate 11 is a heavily doped silicon substrate material, the substrate 11 can be reused as a gate.
[0020] Specifically, the silicon substrate material has good semiconductor properties and can be heavily doped in some cases to achieve specific functions. For example, when it is heavily doped, it can be reused as a gate, which can simplify the structure and reduce costs. The glass substrate may have the characteristics of low cost and good transparency, and is suitable for some application scenarios that require these characteristics. For the gate dielectric layer 12, its material can be silicon nitride or silicon dioxide, or a combination of the two. These two materials have their own advantages in terms of insulation performance, process compatibility, etc.
[0021] Preferably, the thickness of the substrate 11 is 500-800 nm, and the thickness of the gate dielectric layer 12 is 100-300 nm.
[0022] In the embodiment of the present invention, the material of the semiconductor oxide layer 131 is any one of Ga2O3, In2O3 and TiO2, and the material of the metal layer 132 is at least one of Zn and Au.
[0023] In the embodiment of the present invention, the thickness of the semiconductor oxide layer 131 is a, and the thickness of the metal layer 132 is b, wherein the relationship between a and b is as follows: a ≥ 10b; 0 ≤ b ≤ 2nm; wherein the semiconductor oxide layer 131 has a larger thickness ratio, which helps to better control carrier transport. The thinner metal layer 132 can minimize the negative impact on other properties while meeting certain conductivity requirements, such as avoiding problems such as excessive metal ion diffusion.
[0024] In the embodiment of the present invention, the number of layers of the semiconductor oxide layer 131 is c, and the number of layers of the metal layer 132 is d, wherein the relationship between c and d is as follows: c=d+1, 1≤d≤50, and c and d are both positive integers; this means that the number of layers of the semiconductor oxide layer 131 is always one layer more than the number of layers of the metal layer 132. More layers may enhance certain performances, such as increasing the number of carrier transmission channels and improving the stability of the device, but may also increase the manufacturing difficulty and cost. Fewer layers may be more suitable for some simple applications or specific demand scenarios.
[0025] In the embodiment of the present invention, the material of the source electrode 14 and the drain electrode 15 is at least one of molybdenum, titanium, silver, aluminum and copper; the thickness of the source electrode 14 and the drain electrode 15 are both 10-100 nm.
[0026] See also Figure 3 , Figure 3 1 is a flow chart of a method for manufacturing a P-type thin film transistor 100 provided in an embodiment of the present invention; wherein the method comprises: S10 , forming a gate dielectric layer 12 on the substrate 11 .
[0027] Specifically, step S10 also includes: A substrate 11 is provided, wherein the substrate 11 is a heavily doped silicon wafer; Afterwards, a gate dielectric layer 12 is formed on the substrate 11; wherein the gate dielectric layer 12 is SiO2 and has a thickness of 100-300 nm; Finally, the substrate 11 with the gate dielectric layer 12 is rinsed with deionized water and anhydrous ethanol in sequence, then purged with pure nitrogen, and placed in a drying oven for drying.
[0028] S20 , alternately depositing semiconductor oxide layers 131 and metal layers 132 on the gate dielectric layer 12 , with each metal layer 132 inserted between two adjacent semiconductor oxide layers 131 , and finally obtaining a channel layer 13 .
[0029] Specifically, step S20 also includes: The semiconductor oxide layer 131 and the metal layer 132 are alternately deposited on the gate dielectric layer 12 by a physical vapor deposition method, wherein the physical vapor deposition method adopts any one or any combination of electron beam evaporation, molecular beam epitaxial film deposition, DC reactive magnetron sputtering and radio frequency magnetron sputtering.
[0030] Preferably, the channel layer 13 is prepared by magnetron sputtering, and the specific process is as follows: (1) Target material selection: Select materials with a purity of not less than 99.99% as the target material. Select oxide and metal targets. You can also select two or more different target materials. (2) Preparing a channel layer 13 (P-type oxide film) on a substrate: sequentially install an oxide target, a metal target, and a substrate 11 including a gate dielectric layer 12 in a magnetron sputtering chamber. Evacuate to 1*10 -3 Pa, argon and oxygen are introduced to adjust the chamber gas pressure to 0.1-5 Pa; then, appropriate power is selected to complete the ignition of oxide and metal, pre-sputter for 3 minutes, the substrate 11 is turned on to rotate, the oxide and metal are sputtered alternately, and the oxide and metal are deposited alternately to obtain the channel layer 13 as shown in FIG. Figure 2 As shown; The target material in step (1) is alternately sputtered onto the substrate 11 processed in step S10 by magnetron sputtering, wherein the bottom layer and the top layer need to be the semiconductor oxide layer 131, so the cumulative number of deposited thin film layers must be greater than the number of target materials selected in step (1).
[0031] (3) After the channel layer 13 is taken out from the magnetron sputtering chamber, a slow annealing process is performed in an argon atmosphere for 0.5 to 2 hours, followed by natural cooling.
[0032] Preferably, in step S20, the thickness and film forming time of the semiconductor oxide layer 131 or the metal layer 132 are controlled by controlling at least one parameter of the temperature of the substrate 11, the sputtering time, the reaction gas content and the sputtering power.
[0033] Preferably, after the channel layer 13 is prepared, it is necessary to perform a slow annealing treatment on the channel layer 13 to improve the sputtering quality of the channel layer 13 by controlling different atmospheres, holding time, and the like.
[0034] Preferably, in step S20, the material of the semiconductor oxide layer 131 is any one of Ga2O3, In2O3 and TiO2, and the material of the metal layer 132 is at least one of Zn and Au.
[0035] S30 , forming a source electrode 14 and a drain electrode 15 that are spaced apart from each other on the channel layer 13 , wherein the source electrode 14 and the drain electrode 15 are both in contact with a portion of the gate dielectric layer 12 .
[0036] Specifically, step S30 also includes: A source electrode 14 and a drain electrode 15 which are spaced apart from each other are formed on the channel layer 13 by magnetron sputtering. Both the source electrode 14 and the drain electrode 15 are in contact with a portion of the gate dielectric layer 12 .
[0037] The source electrode 14 and the drain electrode 15 are made of at least one of molybdenum, titanium, silver, aluminum and copper; the thickness of the source electrode 14 and the drain electrode 15 are both 10-100 nm.
[0038] At present, the main forms of P-type device preparation are diffusion doping, ion implantation, chemical vapor deposition, physical vapor deposition and molecular beam epitaxy. Among them, diffusion doping and ion implantation have challenges in controlling doping uniformity and depth, especially in nanoscale devices, which require extremely high-precision doping control. At high doping concentrations, ion implantation may introduce lattice damage and affect the electrical properties of the material. Methods such as chemical vapor deposition and molecular beam epitaxy are prone to introduce interface defects and impurities during the deposition process, affecting the performance and reliability of the device. During high-temperature deposition, differences in interface stress and thermal expansion coefficient may cause film cracking or peeling. High-precision preparation methods (such as molecular beam epitaxy) have high equipment costs and slow preparation speeds, which are not conducive to large-scale production. For large-area applications (such as solar cells), it is necessary to reduce production costs and improve preparation efficiency while ensuring material quality.
[0039] The present invention discloses a process for preparing a P-type thin film transistor 100 based on a magnetron sputtering deposition method, which can be applied to the fields of display, flexible technology, etc. The present invention selects a suitable substrate 11, and deposits oxides and metals alternately as a channel layer 13 by magnetron sputtering, and makes a source electrode 14 and a drain electrode 15 through a mask to complete the preparation of the P-type thin film transistor 100. In the preparation of the channel layer 13, different oxides and metals can be selected for alternate sputtering, and the thickness and quantity of different types of thin films can be selected. The post-annealing process can further significantly improve the performance of the thin film transistor, and different times, temperatures, and atmospheres can be selected. Compared with other methods for preparing a P-type thin film transistor 100, this method can be applicable to the doping of different oxides and metals, is simple to operate, can be prepared in batches, and has good controllability.
[0040] The effects of the aforementioned P-type thin film transistor 100 and the method for manufacturing the same are described below through specific embodiments.
[0041] Embodiment 1: Embodiment 1 of the present invention first provides a P-type thin film transistor 100, including a substrate 11, a gate dielectric layer 12, a channel layer 13, a source electrode 14 and a drain electrode 15, wherein the gate dielectric layer 12 is formed on the surface of the substrate 11, and the channel layer 13 is formed on the surface of the gate dielectric layer 12; the source electrode 14 and the drain electrode 15 are both formed on the surface of the channel layer 13 and contact with a portion of the gate dielectric layer 12, and there is a gap between the source electrode 14 and the drain electrode 15; The channel layer 13 includes at least one metal layer 132 and at least two semiconductor oxide layers 131 that are alternately arranged, and each metal layer 132 is inserted between two adjacent semiconductor oxide layers 131 ; at least one semiconductor oxide layer 131 is in contact with the gate dielectric layer 12 .
[0042] In Embodiment 1 of the present invention, the substrate 11 is made of heavily doped silicon material with a thickness of 500 nm; the gate dielectric layer 12 is made of silicon dioxide with a thickness of 300 nm.
[0043] In Example 1 of the present invention, the material of the semiconductor oxide layer 131 is Ga2O3, the thickness of the semiconductor oxide layer 131 is 10 nm, and the number of layers of the semiconductor oxide layer 131 is 5; the material of the metal layer 132 is Zn, the thickness is 1 nm, and the number of layers of the metal layer 132 is 4.
[0044] In the first embodiment of the present invention, the source electrode 14 and the drain electrode 15 are both made of silver, and the thickness of the source electrode 14 and the drain electrode 15 are both 60 nm.
[0045] Specifically, the method for preparing the P-type thin film transistor 100 provided in Embodiment 1 of the present invention is as follows: (1) Selection and treatment of substrate 11: The substrate type of substrate 11 is selected as Si <100> , covered with 300nm thick SiO2, whose resistivity is less than 0.1Ω·cm, the selected substrate 11 is pretreated by ultrasonic cleaning with deionized water and anhydrous ethanol for 2 minutes, then purged with high-purity nitrogen for standby use, and finally placed in a drying oven for drying at 80℃ for 30min for standby use; (2) Target material selection: Zinc and gallium oxide materials with a mass percentage purity of 99.99% are selected as target materials; (3) Fabricating a multilayer thin film of P-type semiconductor material on the substrate 11: The vacuum degree of the substrate 11 is 5×10 -4 Pa, the substrate 11 is not heated, and the rotation speed of the substrate 11 is maintained at 20 rpm; the gallium oxide is sputtered in RF mode, and the zinc is sputtered in DC mode. The sputtering power of gallium oxide is 80 W, and the sputtering power of zinc is 10 W. The deposition rate of both is about 0.1 nm / s. The film thicknesses of zinc and gallium oxide are controlled to be 1 nm and 10 nm, respectively. The gallium oxide layer is deposited first, and then the zinc layer is deposited, and a total of 9 layers are deposited alternately; (4) After the substrate 11 is taken out, it is annealed in an annealing furnace at 900°C in an argon atmosphere for 1 hour. The structure of the channel layer 13 of the manufactured multi-layer thin film is as follows: Figure 2 shown. (5) Using a mask to sputter, a source electrode 14 and a drain electrode 15 are formed; the vacuum degree of the substrate 11 is 5×10 -4 Pa, DC sputtering power is 10w, substrate 11 rotation speed is maintained at 20rpm, and after sputtering for 40S, it is taken out for testing. Its overall structure is as follows Figure 1 shown.
[0046] In this embodiment 1, see Figure 2 As shown, in step (3), the physical vapor deposition sample is deposited successively in the following order: Ga2O3 (10nm) × 5 layers, Zn (1nm) × 4 layers, Ga2O3 (10nm) × 5 layers, the bottom layer and the top layer are both Ga2O3, and a total of 9 thin film layers are deposited on the substrate 11. See also Figure 4 , Figure 4 is a transfer curve diagram of the P-type thin film transistor 100 provided in Example 1 of the present invention; wherein the abscissa is the gate-source voltage Vg, and the ordinate is the drain current I ds , source-drain voltage V ds is -4V.
[0047] Specifically, by Figure 4 It can be seen that at the beginning of the curve, when V g When I is small, ds Almost zero (I ds For 10 -7 A), which corresponds to the cut-off region of the P-type thin film transistor 100, indicating that even if a certain voltage is applied between the drain and the source, almost no current flows through the transistor due to insufficient gate-source voltage. gs Gradually increases, and after reaching a certain threshold voltage, I ds It starts to rise rapidly. The slope of the curve in this stage is large, showing an approximately linear growth trend, which means that the P-type thin film transistor 100 has entered the linear region. At this time, the gate-source voltage has a strong control effect on the drain current, and the drain current increases significantly with the increase of the gate-source voltage. g (At this time V g Less than -20V), I ds The growth rate will gradually slow down, and the curve will eventually flatten and enter the saturation region. In this region, the drain current (I ds For 10 -3 ~10 -2 A) basically remains stable and no longer changes with V gAt this time, the conductive channel of the P-type thin film transistor 100 has been fully formed, and the current is mainly limited by factors such as the channel resistance.
[0048] Therefore, by Figure 4 It can be seen that the P-type thin film transistor 100 provided in Embodiment 1 of the present invention has strong repeatability and can control the composition and thickness of different thin film layers. Compared with the P-type thin film transistor 100 prepared by other methods, it has the advantages of low cost, high speed and strong stability.
[0049] The P-type thin film transistor 100 and the preparation method thereof provided by the present invention can select a silicon substrate or a glass substrate, and different target materials and metals can be selected for alternate sputtering during the sputtering process, and the film thickness or the number of films can be selected. The method is simpler to operate than other methods, can be mass-produced over a large area, has strong controllability, can prepare P-type thin film transistors 100 of different oxides, and can be applied to display, flexible devices and other fields.
[0050] In the embodiment of the present invention, magnetron sputtering technology is divided into two types: direct current and radio frequency. This method uses positive ions in argon plasma to bombard a solid target, so that neutral atoms of the target material are sputtered and deposited on a substrate to form a thin film. This process has the advantages of low operating temperature and high speed, and is particularly suitable for preparing materials with special properties, such as ultra-thin film systems required in electronic devices and flexible electronic devices. Reactive magnetron sputtering adjusts the sputtering process by introducing reactive gases, thereby accurately controlling the composition and properties of the film to adapt it to different application requirements. By changing the magnetron sputtering parameters to control the P-type thin film transistor 100 with different performances, this technology is easy to operate, does not have special requirements for the substrate 11 and experimental conditions, and the generated film is well bonded to the substrate 11, has high purity, and has high experimental repeatability. It can accurately control the composition and thickness of the film, so it is of great significance in the preparation and research of the P-type thin film transistor 100. In addition, compared with the traditional physical method, this method overcomes the problems of cumbersome process, poor bonding, and poor stability when making the P-type thin film transistor 100, and has brought significant help to the progress of the P-type thin film transistor 100.
[0051] Compared with the prior art, the present invention has the following obvious outstanding substantive features and significant advantages: First, the present invention uses a magnetron sputtering method to prepare a P-type thin film transistor 100, and controls the device performance and application field by controlling parameters such as the thickness and quality of the single-layer film, thereby overcoming the difficulties in preparing and poor performance of existing oxide thin film transistors. The operation is simple, and the prepared thin film material has good performance, good material adhesion and is easy to industrialize. Second, the P-type thin film transistor 100 prepared by the multi-layer alternating sputtering method selected by the present invention optimizes the conductance path by inserting an ultra-thin metal layer 132, reduces the effect of interface scattering on carrier mobility; reduces defects and lowers potential barriers, reduces the possibility of carrier recombination, and improves mobility. Therefore, by sputtering multiple layers of metal, interface scattering is reduced and a conductance path is formed, making carrier migration smoother and improving conductivity; defect compensation and interface state passivation reduce carrier recombination and increase the number of effective carriers; band alignment and energy level matching optimize the carrier transmission path, reduce energy loss, and improve mobility. The low formation energy and atomic radius matching of metal element doping further improve the doping efficiency and material quality, thereby improving the performance of the P-type thin film transistor 100.
[0052] Third, in the P-type thin film transistor 100 prepared by the present invention, suitable metal elements are doped into the multilayer semiconductor oxide material to prepare the channel layer 13. These metal elements replace the metal elements of the oxide in the lattice to form shallow acceptors at the top of the valence band. Carriers migrate freely under the action of the electric field, thereby exhibiting P-type conductive characteristics. Compared with other doping methods, alternating sputtering can better control the uniformity and doping concentration of each layer; at the same time, the channel layer 13 prepared by the present invention is subsequently annealed, which can further improve the electrical performance of the P-type thin film transistor 100.
[0053] Fourthly, the channel layer 13 obtained in the present invention has good adhesion to the substrate 11, the film quality of the channel layer 13 is uniform, the experimental repeatability is good, and the composition and thickness of the channel layer 13 are controllable.
[0054] Fifth, compared with other methods for making multilayer membrane structures, the present invention has the advantages of fast speed, low temperature, strong controllability, high purity, and no cross contamination.
[0055] In summary, different from the prior art, the present invention provides a P-type thin film transistor 100 and a preparation method thereof, wherein the P-type thin film transistor 100 includes a substrate 11, a gate dielectric layer 12, a channel layer 13, a source electrode 14 and a drain electrode 15, wherein the gate dielectric layer 12 is formed on the surface of the substrate 11, and the channel layer 13 is formed on the surface of the gate dielectric layer 12; the source electrode 14 and the drain electrode 15 are both formed on the surface of the channel layer 13 and are in contact with a portion of the gate dielectric layer 12, and there is a gap between the source electrode 14 and the drain electrode 15, wherein the channel layer 13 includes at least one metal layer 132 and at least two semiconductor oxide layers 131 alternately arranged, and each metal layer 132 is inserted between two adjacent semiconductor oxide layers 131; and at least one semiconductor oxide layer 131 is in contact with the gate dielectric layer 12. The present invention arranges the channel layer 13 in the P-type thin film transistor 100 into a multilayer structure formed by alternating semiconductor oxide layers 131 and metal layers 132, and inserts the metal layer 132 between two adjacent semiconductor oxide layers 131 to optimize the conduction path, reduce the influence of interface scattering on carrier mobility, reduce the possibility of carrier recombination to improve mobility, and thus improve the switching ratio of the P-type thin film transistor 100, and ultimately improve the electrical performance of the P-type thin film transistor 100.
[0056] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.
[0057] The above embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.
Claims
1. A P-type thin film transistor, It is characterized in that The invention comprises a substrate, a gate dielectric layer, a channel layer, a source electrode and a drain electrode, wherein the gate dielectric layer is formed on the surface of the substrate, and the channel layer is formed on the surface of the gate dielectric layer; the source electrode and the drain electrode are both formed on the surface of the channel layer and contact with a part of the gate dielectric layer, and there is a gap between the source electrode and the drain electrode; The channel layer includes at least one metal layer and at least two semiconductor oxide layers that are alternately arranged, each of the metal layers is inserted between two adjacent semiconductor oxide layers; and at least one of the semiconductor oxide layers is in contact with the gate dielectric layer.
2. The P-type thin film transistor according to claim 1, It is characterized in that The material of the semiconductor oxide layer is Ga 2 O 3 、In 2 O 3 and TiO 2 Any one of the above, wherein the material of the metal layer is at least one of Zn and Au.
3. The P-type thin film transistor according to claim 1, It is characterized in that The thickness of the semiconductor oxide layer is a, and the thickness of the metal layer is b, wherein the relationship between a and b is as follows: a≥10b; 0≤b≤2nm.
4. The P-type thin film transistor according to claim 1, It is characterized in that The number of layers of the semiconductor oxide layer is c, and the number of layers of the metal layer is d, wherein the relationship between c and d is as follows: c=d+1, 1≤d≤50, and c and d are both positive integers.
5. The P-type thin film transistor according to claim 1, It is characterized in that The base is made of silicon substrate material, and the gate dielectric layer is made of at least one of silicon nitride and silicon dioxide.
6. The P-type thin film transistor according to claim 1, It is characterized in that The source electrode and the drain electrode are made of at least one of molybdenum, titanium, silver, aluminum and copper.
7. A method for preparing a P-type thin film transistor according to any one of claims 1 to 6, It is characterized in that The method comprises: S10, forming the gate dielectric layer on the substrate; S20, alternately depositing the semiconductor oxide layer and the metal layer on the gate dielectric layer, wherein each metal layer is inserted between two adjacent semiconductor oxide layers, and finally obtaining the channel layer; S30, forming the source electrode and the drain electrode spaced apart from each other on the channel layer, wherein both the source electrode and the drain electrode are in contact with a portion of the gate dielectric layer.
8. The method for preparing a P-type thin film transistor according to claim 7, It is characterized in that In the step S20, the semiconductor oxide layer and the metal layer are alternately deposited on the gate dielectric layer by a physical vapor deposition method, and the physical vapor deposition method adopts any one or any combination of electron beam evaporation, molecular beam epitaxial film deposition, DC reactive magnetron sputtering and radio frequency magnetron sputtering methods.
9. The method for preparing a P-type thin film transistor according to claim 7, It is characterized in that In the step S20, the thickness and film forming time of the semiconductor oxide layer or the metal layer are controlled by controlling at least one parameter of the temperature of the substrate, the sputtering time, the reaction gas content and the sputtering power.
10. The method for preparing a P-type thin film transistor according to claim 7, It is characterized in that In the step S20, the material of the semiconductor oxide layer is Ga 2 O 3 、In 2 O 3 and TiO 2 Any one of the above, wherein the material of the metal layer is at least one of Zn and Au.