TOPCON battery and preparation method thereof
By setting up a multi-layer passivation structure of tunneling oxide layer, intrinsic polysilicon layer and doped polysilicon layer on the back of the TOPCON battery, the problem that traditional doped polysilicon layer cannot guarantee high doping concentration and boron atom penetration is solved, and the problem of the traditional doped polysilicon layer cannot guarantee high doping concentration and boron atom penetration is improved. The battery conversion efficiency and double-sided rate extend the battery life.
Patent Information
- Application Number
- CN202410927289.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-19
AI Technical Summary
In the existing TOPCON batteries, the traditional doped polysilicon layer is subject to boron doping characteristics, and cannot guarantee the high doping concentration in polysilicon, and boron atoms may penetrate the silicon oxide layer, affecting the double-sided ratio and conversion efficiency of the battery. .
The multi-layer passivation structure is adopted to set a tunneling oxide layer, an intrinsic polysilicon layer, a doped polysilicon layer and a barrier layer on the back of the silicon wafer. It is prepared by low-pressure chemical vapor deposition method and low-temperature atomic layer deposition method to control the barrier layer's Thickness and density prevent the expansion of boron atoms, form a multi-layer passivation contact structure, and improve the conversion efficiency and double-sided rate of the battery.
It achieves higher battery conversion efficiency and double-sided rate, reduces the thickness of the doped polysilicon layer, enhances the passivation effect, and extends the service life and stability of the battery.
Smart Images

Figure CN118983352A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of solar cells, and more specifically, to a TOPCON cell and a preparation method thereof. Background Art
[0002] TOPCON cell, the full name of which is Tunnel Oxide Passivated Contact solar cell, has made remarkable achievements in improving photoelectric conversion efficiency and reducing energy loss.
[0003] TOPCON cells use the principle of selective carriers. By preparing an ultra-thin layer of silicon oxide on the back of the silicon substrate cell and depositing a thin layer of doped silicon, a passivation contact structure is formed. This structure effectively prevents electrons from moving to the surface of the silicon substrate, thereby greatly reducing the surface recombination effect and improving the photoelectric conversion efficiency of the cell. In addition to the efficient passivation contact structure, TOPCON cells also deposit an oxide layer on the surface of the silicon substrate, which not only prevents the loss of electrons, but also effectively reduces the loss of low-energy photons, further improving the photoelectric conversion efficiency of TOPCON cells. The technical features also include high conversion efficiency, low light loss, and low surface recombination rate. Compared with traditional silicon-based solar cells, TOPCON cells have higher photoelectric conversion efficiency and can convert more solar energy into electrical energy. At the same time, its low light loss and low surface recombination rate also give the cell a longer service life and higher stability. Therefore, TOPCON cell technology has high industrialization value and power generation value.
[0004] At present, in the existing TOPCON cells, the traditional doped polysilicon layer is restricted by the characteristics of boron doping, and it is impossible to ensure a high doping concentration in the polysilicon, nor to ensure that the boron atoms will not penetrate the silicon oxide layer into the silicon substrate. Furthermore, the parasitic light absorption of the highly doped polysilicon layer increases, affecting the bifaciality of the cell.
[0005] Therefore, there is an urgent need to provide a TOPCON battery and a preparation method thereof that can improve the battery conversion efficiency and bifaciality. Summary of the invention
[0006] In view of this, in one aspect, the present invention provides a TOPCON battery, comprising: a silicon wafer;
[0007] It also includes a tunneling oxide layer disposed on a first surface of the silicon wafer along a first direction, an intrinsic polysilicon layer, a doped polysilicon layer and an anti-reflection layer stacked in sequence on a side of the tunneling oxide layer away from the first surface, the first direction being the thickness direction of the silicon wafer; the first surface being the back side of the battery;
[0008] Along the first direction, a barrier layer is further provided between the intrinsic polysilicon layer and the doped polysilicon layer, and the thickness of the barrier layer is less than the thickness of the doped polysilicon layer.
[0009] Optionally, the silicon wafer is a P-type silicon wafer, and the material of the barrier layer is aluminum oxide; the silicon wafer also includes a second surface, which is the front side of the battery; along the first direction, the second surface is sequentially stacked with an N-type emitter, a silicon oxide film and an anti-reflection layer.
[0010] Optionally, along the first direction, the thickness of the barrier layer is a, 0.1 nm≤a≤1.5 nm.
[0011] Optionally, along the first direction, the thickness of the tunnel oxide layer is c, 1.5nm≤c≤3.0nm; the thickness of the intrinsic polysilicon layer is b, 40nm≤b≤70nm; and the thickness of the doped polysilicon layer is d, 20nm≤d≤50nm.
[0012] On the other hand, the present invention also provides a method for preparing a TOPCON battery, which is applicable to the above-mentioned TOPCON battery, comprising the steps of:
[0013] Alkali polishing;
[0014] Preparation of tunnel oxide layer by low pressure chemical vapor deposition;
[0015] Preparation of intrinsic polysilicon layer by low pressure chemical vapor deposition;
[0016] Preparation of barrier layer by low temperature atomic layer deposition;
[0017] Preparation of doped polysilicon layer by plasma enhanced chemical vapor deposition;
[0018] annealing;
[0019] The anti-reflection layer was prepared by plasma enhanced chemical vapor deposition.
[0020] Optionally, the intrinsic polysilicon layer is prepared by low pressure chemical vapor deposition, comprising the steps of:
[0021] Deposition is started at a first growth temperature for a first time and is increased to a second growth temperature for a second time; the first growth temperature C1, 500°C≤C1≤600°C; the second growth temperature C2, 570°C≤C2≤630°C; the first time T1, 565s≤T1≤965s; the second time T2, 435s≤T2≤935s.
[0022] Optionally, the barrier layer is prepared by low temperature atomic layer deposition, comprising the steps of:
[0023] The temperature rises to 150℃-225℃;
[0024] Evacuate to a pressure of 0.05-0.3 mTorr;
[0025] A mixed gas of ozone and water vapor and trimethylaluminum are introduced.
[0026] Optionally, the tunnel oxide layer is deposited by low pressure chemical vapor deposition, including the following conditions: temperature of 550° C.-650° C., and time of 350 s-900 s.
[0027] Optionally, the doped polysilicon layer is prepared by plasma enhanced chemical vapor deposition, including the following conditions: the reaction gases are silane and borane, the gas pressure is 70Pa-120Pa, and the temperature is 220°C-400°C.
[0028] Optionally, annealing includes conditions: temperature of 880°C-960°C, treatment for 20min-40min.
[0029] Compared with the prior art, the TOPCON battery and the preparation method thereof provided by the present invention achieve at least the following beneficial effects:
[0030] The TOPCON cell provided by the present invention comprises a silicon wafer and a tunneling oxide layer arranged on a first surface of the silicon wafer along a first direction, an intrinsic polysilicon layer, a doped polysilicon layer and an anti-reflection layer which are sequentially stacked and arranged on a side of the tunneling oxide layer away from the first surface, and a barrier layer is further arranged between the intrinsic polysilicon layer and the doped polysilicon layer along the first direction, the barrier layer passivates the surface of the intrinsic polysilicon layer, realizes hole selective transmission, forms a certain barrier to the subsequent expansion of boron atoms, and reduces the diffusion depth; the barrier layer and the intrinsic polysilicon layer form a multi-layer passivation structure, further enhances the passivation effect, and improves the conversion efficiency of the cell; the thickness of the barrier layer The thickness of the doped polysilicon layer is less than that of the doped polysilicon layer, and the thinner barrier layer can achieve a high probability of tunnel effect, further improving the battery conversion efficiency and the bifaciality level; the setting of the intrinsic polysilicon layer reduces the thickness of the doped polysilicon in the existing battery structure to a certain extent, improves the back efficiency of the TOPCON battery, and improves the bifaciality level; in the TOPCON battery preparation method provided by the present invention, the intrinsic polysilicon layer and the doped polysilicon layer adopt different manufacturing processes to achieve different densities, improve the passivation effect, and enhance the blocking effect to boron; the barrier layer is prepared by low-temperature atomic layer deposition method, so as to better realize the control of the thickness of the barrier layer.
[0031] Of course, any product implementing the present invention does not necessarily need to achieve all of the technical effects described above at the same time.
[0032] Further features and advantages of the present invention will become apparent from the following detailed description of exemplary embodiments of the present invention with reference to the attached drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention.
[0034] Figure 1 This is a schematic diagram of a TOPCON battery structure provided by the present invention;
[0035] Figure 2 This is another schematic diagram of the TOPCON battery structure provided by the present invention;
[0036] Figure 3 This is a flow chart of a TOPCON battery preparation method provided by the present invention;
[0037] 100-battery, 1-silicon wafer, 11-first surface, 12-second surface, 2-tunneling oxide layer, 3-intrinsic polysilicon layer, 4-barrier layer, 5-doped polysilicon layer, 6-anti-reflection layer, 7-N-type emitter, 8-silicon oxide film, y-first direction. DETAILED DESCRIPTION
[0038] Various exemplary embodiments of the present invention will now be described in detail with reference to the accompanying drawings. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present invention unless otherwise specifically stated.
[0039] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the invention, its application, or uses.
[0040] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0041] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0042] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0043] Combination Figure 1 , the present invention provides a TOPCON battery, comprising: a silicon wafer 1;
[0044] It also includes a tunneling oxide layer 2 disposed on a first surface 11 of the silicon wafer 1 along a first direction y, an intrinsic polysilicon layer 3, a doped polysilicon layer 5 and an anti-reflection layer 6 stacked in sequence on a side of the tunneling oxide layer 2 away from the first surface 11, the first direction y being the thickness direction of the silicon wafer 1; the first surface 11 being the back side of the battery 100;
[0045] Along the first direction y, a barrier layer 4 is further provided between the intrinsic polysilicon layer 3 and the doped polysilicon layer 5 , and the thickness of the barrier layer 4 is smaller than the thickness of the doped polysilicon layer 5 .
[0046] Specifically, the present invention provides a TOPCON battery, comprising: a silicon wafer 1; a tunneling oxide layer 2 arranged on a first surface 11 of the silicon wafer 1 along a first direction y, an intrinsic polysilicon layer 3, a doped polysilicon layer 5 and an anti-reflection layer 6 stacked in sequence on a side of the tunneling oxide layer 2 away from the first surface 11, the first direction y being the thickness direction of the silicon wafer 1; the first surface 11 being the back side of the battery 100; a barrier layer 4 is further arranged between the intrinsic polysilicon layer 3 and the doped polysilicon layer 5 along the first direction y, and the barrier layer 4 is arranged between the intrinsic polysilicon layer 3 and the doped polysilicon layer 5. A multi-layer passivation contact structure is arranged on the back side of the cell 100 to further enhance the passivation effect, reduce the doping concentration of the doped polysilicon layer 5, and reduce the parasitic absorption of light on the first surface 11. In addition, the barrier layer 4 increases the passivation effect at the interface of the intrinsic polysilicon layer 3, increases the opening voltage gain of the first surface 11, improves the efficiency of the first surface 11, and improves the bifaciality of the battery 100. The thickness of the barrier layer 4 is less than the thickness of the doped polysilicon layer 5. The thinner barrier layer 4 has a higher tunneling characteristic and has good hole selection characteristics and passivation effect.
[0047] It should be noted that the material of the tunnel oxide layer 2 may be silicon oxide (SiOx), and the tunnel oxide layer 2 may realize hole selective transmission with doped polysilicon, avoid contact with the metal gate line groove, and reduce damage to the passivation layer.
[0048] It should be noted that an intrinsic polysilicon layer 3 and a doped polysilicon layer 5 are arranged on the side of the tunneling oxide layer 2 away from the first surface 11, and a barrier layer 4 is arranged between the intrinsic polysilicon layer 3 and the doped polysilicon layer 5 to form a multi-layer passivation contact structure, which further enhances the passivation effect and improves the battery conversion efficiency.
[0049] It should be noted that the material of the anti-reflection layer 6 is generally silicon nitride (SiNx), which can reduce the reflectivity of light, improve the transmittance of light, and increase the light absorptivity of the first surface 11 of the battery 100 .
[0050] It can be understood that the TOPCON cell 100 provided by the present invention includes a silicon wafer 1 and a tunneling oxide layer 2 arranged on the first surface 11 of the silicon wafer 1 along the first direction y, an intrinsic polysilicon layer 3, a doped polysilicon layer 5 and an anti-reflection layer 6 are stacked in sequence on the side of the tunneling oxide layer 2 away from the first surface 11, and a barrier layer 4 is also provided between the intrinsic polysilicon layer 3 and the doped polysilicon layer 5 along the first direction y. The barrier layer 4 passivates the surface of the intrinsic polysilicon layer 3 to achieve selective hole transmission, thereby forming a certain obstacle to the subsequent expansion of boron atoms and reducing the diffusion depth; the barrier layer 4 and the intrinsic polysilicon layer 3 form a multi-layer passivation structure to further enhance the passivation effect and improve the battery conversion efficiency; the thickness of the barrier layer 4 is less than the thickness of the doped polysilicon layer 5, and the thinner barrier layer 4 can achieve a high probability of tunnel effect, enhance the tunneling characteristics, and further improve the battery conversion efficiency; the setting of the intrinsic polysilicon layer 3 reduces the thickness of the doped polysilicon in the existing battery structure to a certain extent, improves the back efficiency of the TOPCON battery, and improves the bifaciality level.
[0051] Table 1 is a comparison table of TOPCON battery bifaciality, where the experimental group corresponds to the TOPCON battery provided in this embodiment, and the control group corresponds to the TOPCON battery of the prior art;
[0052] Table 1 TOPCON battery bifaciality comparison table
[0053]
[0054] A TOPCON cell provided by the present invention comprises: a silicon wafer 1; a tunneling oxide layer 2 arranged on a first surface 11 of the silicon wafer 1 along a first direction y, an intrinsic polysilicon layer 3, a doped polysilicon layer 5 and an anti-reflection layer 6 stacked in sequence on a side of the tunneling oxide layer 2 away from the first surface 11, the first direction y being the thickness direction of the silicon wafer 1; the first surface 11 being the back side of the cell 100; a barrier layer 4 is further arranged between the intrinsic polysilicon layer 3 and the doped polysilicon layer 5 along the first direction y, and the thickness of the barrier layer 4 is less than the thickness of the doped polysilicon layer 5; exemplary, the present application conducts comparative experiments on the above embodiments, as shown in Table 1, a TOPCON cell provided by the present invention is compared with a TOPCON cell of the prior art in which an intrinsic polysilicon layer and a barrier layer are not arranged on the back side. The comparison group (TOPCON battery of the prior art) had a battery efficiency of 21.88 on the back, and a battery efficiency of 26.14 on the front; the experimental group (TOPCON battery provided by the present invention) had a battery efficiency of 22.05 on the back, and a battery efficiency of 26.25 on the front; the comparison group (TOPCON battery of the prior art) had an open circuit voltage of 0.7369 on the back, and an open circuit voltage of 0.7364 on the front; the experimental group (TOPCON battery provided by the present invention) had an open circuit voltage of 0.7376 on the back, and an open circuit voltage of 0.7374 on the front; the comparison group (TOPCON battery of the prior art) had a short circuit current of 11.480 on the back, and a short circuit current of 1 3.760; the short-circuit current of the back of the experimental group (TOPCON battery provided by the present invention) is 11.827, and the short-circuit current of the front is 14.070; the filling factor of the back of the comparison group (TOPCON battery provided by the prior art) is 85.41, and the filling factor of the front is 85.18; the filling factor of the back of the experimental group (TOPCON battery provided by the present invention) is 85.47, and the filling factor of the front is 85.60; the series resistance of the back of the comparison group (TOPCON battery provided by the prior art) is 0.0010, and the series resistance of the front is 0.0009; the series resistance of the back of the experimental group (TOPCON battery provided by the present invention) is 0.001, and the series resistance of the front is 0.0009 ; The parallel resistance of the back of the comparison group (TOPCON battery of the prior art) is 4390, and the parallel resistance of the front is 4154; the parallel resistance of the back of the experimental group (TOPCON battery provided by the present invention) is 3409, and the parallel resistance of the front is 3563; the reverse leakage current of the back of the comparison group (TOPCON battery of the prior art) is 0.008, and the reverse leakage current of the front is 0.062; the reverse leakage current of the back of the experimental group (TOPCON battery provided by the present invention) is 0.009, and the reverse leakage current of the front is 0.055; the bifaciality of the comparison group (TOPCON battery of the prior art) is 83.72%; the bifaciality of the experimental group (TOPCON battery provided by the present invention) is 84.00%; In summary, the TOPCON cell 100 provided by the present invention comprises a silicon wafer 1 and a tunneling oxide layer 2 arranged on a first surface 11 of the silicon wafer 1 along a first direction y, an intrinsic polysilicon layer 3, a doped polysilicon layer 5 and an anti-reflection layer 6 which are sequentially stacked and arranged on a side of the tunneling oxide layer 2 away from the first surface 11, and a barrier layer 4 is further arranged between the intrinsic polysilicon layer 3 and the doped polysilicon layer 5 along the first direction y, the barrier layer 4 passivates the surface of the intrinsic polysilicon layer 3, realizes hole selective transmission, forms a certain barrier to the subsequent expansion of boron atoms, and reduces the diffusion depth; the barrier layer 4 and the intrinsic polysilicon layer 3 form a multi-layer passivation structure, further enhances the passivation effect, and improves the cell conversion efficiency; the thickness of the barrier layer 4 is less than the thickness of the doped polysilicon layer 5, and the thinner barrier layer 4 can achieve a high probability of tunnel effect, enhance the tunneling characteristics, and further improve the cell conversion efficiency; the setting of the intrinsic polysilicon layer 3 reduces the thickness of the doped polysilicon in the existing cell structure to a certain extent, improves the back efficiency of the TOPCON cell, and improves the bifaciality level. .
[0055] Demonstratively, a simple optical simulation was performed on the TOPCON cell provided by the present invention on a PV lighthouse, and the TOPCON cell provided by the present invention was tested and simulated using the AM1.5 solar spectrum, and compared with the cell of the prior art (a TOPCON cell without an intrinsic polysilicon layer and a barrier layer on the back). The results showed that the TOPCON cell provided by the present invention had increased JG light absorption.
[0056] In some optional embodiments, the silicon wafer 1 is a P-type silicon wafer, and the material of the barrier layer 4 is aluminum oxide; in some optional embodiments, referring to Figure 2 The silicon wafer 1 also includes a second surface 12, which is the front side of the battery 100; along the first direction y, the second surface 12 is stacked with an N-type emitter 7, a silicon oxide film 8 and an anti-reflection layer 6 in sequence.
[0057] It should be noted that the barrier layer 4 is disposed on the back side of the TOPCON battery 100. Since the aluminum oxide film layer structure is negatively charged, it can be disposed on the back side only when the silicon wafer 1 is a P-type silicon wafer, thereby realizing a multi-layer passivation contact structure, enhancing the passivation effect, and further improving the bifaciality.
[0058] It should be noted that the silicon wafer 1 also includes a second surface 12, which is the front side of the battery 100; along the first direction y, the second surface 12 is stacked with an N-type emitter 7, a silicon oxide film 8 and an anti-reflection layer 6 in sequence; the phosphorus-doped N-type region is introduced into the second surface 12 of the P-type silicon wafer 1 (the front side of the battery 100) to form an N-type emitter 7; the N-type emitter 7 layer forms a PN junction with the P-type silicon wafer 1. When sunlight irradiates the solar cell, the energy of the photon will excite the electrons in the P-type emitter layer, causing it to transition to the conduction band to form free electrons. At the same time, the energy of the photon will also excite the holes in the P-type emitter layer, causing it to transition to the valence band to form free holes. In this way, the P-type emitter layer injects electrons and holes into the PN junction. Due to the existence of the PN junction, the electrons and holes will be affected by the electric field force and separated into different areas to form a potential difference. In this way, an electric field is generated, causing the electrons and holes to move in opposite directions in the PN junction to form a current.
[0059] In some optional embodiments, referring to Figure 1 , along the first direction y, the thickness of the barrier layer 4 is a, 0.1nm≤a≤1.5nm.
[0060] Optionally, along the first direction y, the thickness a of the barrier layer 4 can be 0.1 nm, 0.15 nm, 0.2 nm, 0.23 nm, 0.27 nm, 0.3 nm, 0.34 nm, 0.38 nm, 0.4 nm, 0.45 nm, 0.47 nm, 0.5 nm, 0.56 nm, 0.59 nm, 0.6 nm, 0.61 nm, 0.67 nm, 0.7 nm, 0.74 nm, 0.76 nm, 0.8 nm, 0.81 nm, 0.88 nm, 0.9 nm, 0.93 nm, 0.98 nm, 1.0 nm, 1.07 nm, 1.09 nm, 1.1 nm, 1.16 nm, 1.18 nm, 1.2 nm, 1.24 nm, 1.28 nm, 1.3 nm, 1.35 nm, 1.38 nm, 1.4 nm, 1.5 45nm, 1.47nm, 1.5nm; when a<0.1nm, along the first direction y, the thickness of the blocking layer 4 is too small. On the one hand, the preparation is difficult and the production cost is high; on the other hand, the passivation effect of the too thin blocking layer 4 is also poor, and the effect of improving the battery efficiency cannot be achieved; when a>1.5nm, along the first direction y, the thickness of the blocking layer 4 is too large, and the tunneling characteristics of the too thick blocking layer 4 are relatively small, which affects its passivation effect; so when 0.1nm≤a≤1.5nm, along the first direction y, the thickness of the blocking layer 4 is moderate, which can maintain good tunneling characteristics and realize selective hole transmission, and can also maintain good passivation effect, passivate the surface of the intrinsic polysilicon layer 3, increase the passivation effect at the interface of the intrinsic polysilicon layer 3, and increase the first surface 11 opening voltage gain, thereby improving the efficiency of the first surface 11, and thus improving the bifaciality of the battery 100.
[0061] Optionally, along the first direction y, the thickness a of the barrier layer 4 may also be 0.1 nm≤a≤0.65 nm, 0.5 nm≤a≤0.8 nm, 0.7 nm≤a≤1.26 nm, 0.95 nm≤a≤1.4 nm, 1.2 nm≤a≤1.45 nm and 1.36 nm≤a≤1.5 nm.
[0062] In some optional embodiments, referring to Figure 1 Along the first direction y, the thickness of the tunnel oxide layer 2 is c, 1.5nm≤c≤3.0nm; the thickness of the intrinsic polysilicon layer 3 is b, 40nm≤b≤70nm; and the thickness of the doped polysilicon layer 5 is d, 20nm≤d≤50nm.
[0063] Optionally, along the first direction y, the thickness c of the tunnel oxide layer 2 can be 1.5nm, 1.54nm, 1.58nm, 1.6nm, 1.64nm, 1.67nm, 1.7nm, 1.76nm, 1.78nm, 1.8nm, 1.83nm, 1.87nm, 1.9nm, 1.94nm, 1.98nm, 2.0nm, 2.05nm, 2.08nm, 2.1nm, 2.15nm, 2.19nm, 2.2nm, 2.23nm, 2.3nm, 2.35nm, 2.38nm, 2.4nm, 2.43nm, 2.45nm, 2.5nm, 2.6nm, 2.67nm, 2.7nm, 2.76nm, 2.8nm, 2.9nm, 2.95nm and 3.0nm; c<1.5nm m, along the first direction y, the thickness of the tunneling oxide layer 2 is relatively small. A too thin tunneling oxide layer 2 has a small blocking effect on boron, and the quality of the preparation cannot be effectively guaranteed. There may be many defects and pores in the tunneling oxide layer 2, which will cause a short circuit in the battery and greatly reduce the degree of recombination of carriers on the rear surface of the solar cell; when c>3.0nm, along the first direction y, the thickness of the tunneling oxide layer 2 is relatively large. A too thick tunneling oxide layer 2 will seriously hinder the migration of electrons, and the tunneling effect will be reduced, thereby increasing the series resistance of the battery, and the fill factor and current of the battery will be affected and reduced, affecting the battery conversion efficiency; therefore, 1.5nm≤c≤3.0nm, along the first direction y, the thickness of the tunneling oxide layer 2 is moderate, and it has a good effect of blocking the expansion of boron, and neither short circuit of the battery nor hindering the migration of electrons will occur.
[0064] Optionally, along the first direction y, the thickness b of the intrinsic polysilicon layer 3 may be 40nm, 41nm, 42nm, 43nm, 44nm, 45nm, 46nm, 47nm, 48nm, 49nm, 50nm, 51nm, 52nm, 53nm, 54nm, 55nm, 56nm, 57nm, 58nm, 59nm, 60nm, 61nm, 62nm, 63nm, 64nm, 65nm, 66nm, 67nm, 68nm, 69nm, nm and 70nm; when b<40nm, along the first direction y, the thickness of the intrinsic polysilicon layer 3 is small, and the doping concentration of the polysilicon layer of the battery 100 is high, which will affect the light absorption rate; when b>70nm, along the first direction y, the thickness of the intrinsic polysilicon layer 3 is large, and the excessively thick intrinsic polysilicon layer 3 affects its passivation effect; therefore, when 40nm≤b≤70nm, along the first direction y, the thickness of the intrinsic polysilicon layer 3 is appropriate, which can not only reduce the doping concentration of the polysilicon layer of the battery 100, but also ensure the passivation effect.
[0065] Optionally, along the first direction y, the thickness d of the doped polysilicon layer 5 can be 20nm, 21nm, 22nm, 23nm, 24nm, 25nm, 27nm, 29nm, 30nm, 32nm, 33nm, 35nm, 37nm, 38nm, 39nm, 40nm, 41nm, 42nm, 43nm, 44nm, 45nm, 46nm, 47nm, 48nm, 49nm and 50nm; when d<20nm, along the first direction y, the thickness d of the doped polysilicon layer 5 can be 20nm, 21nm, 22nm, 23nm, 24nm, 25nm, 27nm, 29nm, 30nm, 32nm, 33nm, 35nm, 37nm, 38nm, 39nm, 40nm, 41nm, 42nm, 43nm, 44nm, 45nm, 46nm, 47nm, 48nm, 49nm and 50nm; In the direction y, the thickness of the doped polysilicon layer 5 is too small, the thickness of the polysilicon layer of the battery 100 is small, and the passivation effect is poor; when d>40nm, along the first direction y, the thickness of the doped polysilicon layer 5 is large, the doping concentration of the polysilicon layer of the battery 100 is high, the parasitic absorption of the back light increases, affecting the bifaciality of the battery 100; therefore, when 20nm≤d≤50nm, along the first direction y, the thickness of the doped polysilicon layer 5 is moderate, the doping concentration of the polysilicon layer of the entire battery 100 is moderate, and the passivation effect is better.
[0066] Optionally, along the first direction y, the thickness c of the tunneling oxide layer 2 can be 1.5nm≤c≤3.0nm, 1.5nm≤c≤1.95nm, 1.76nm≤c≤2.3nm, 2.15nm≤c≤2.6nm and 2.5nm≤c≤3.0nm; the thickness b of the intrinsic polysilicon layer 3 can be 40nm≤b≤51.5nm, 49.6nm≤b≤55nm, 53.4nm≤b≤62nm, 61.4nm≤b≤66nm, 65.6nm≤b≤67.8nm and 66nm≤b≤70nm; the thickness d of the doped polysilicon layer 5 can be 20nm≤d≤25.8nm, 26nm≤d≤32.5nm, 28nm≤d≤37nm, 32nm≤d≤45nm and 39nm≤d≤50nm.
[0067] Based on the same invention idea, refer to Figure 3 The present invention also provides a method for preparing a TOPCON battery 100, which is applicable to the above-mentioned TOPCON battery 100, comprising the steps of:
[0068] S1: alkali polishing;
[0069] S2: preparing tunnel oxide layer 2 by low pressure chemical vapor deposition method;
[0070] S3: preparing an intrinsic polysilicon layer 3 by low pressure chemical vapor deposition;
[0071] S4: preparing barrier layer 4 by low temperature atomic layer deposition;
[0072] S5: preparing a doped polysilicon layer 5 by plasma enhanced chemical vapor deposition;
[0073] S6: annealing;
[0074] S7: preparing the anti-reflection layer 6 by plasma enhanced chemical vapor deposition.
[0075] Specifically, the present invention also provides a method for preparing a TOPCON battery, which is applicable to the above-mentioned TOPCON battery, comprising the steps of:
[0076] S1: Alkali polishing; Alkali polishing generally uses NaOH or KOH solution;
[0077] S2: preparing tunnel oxide layer 2 by low pressure chemical vapor deposition method;
[0078] S3: preparing an intrinsic polysilicon layer 3 by low pressure chemical vapor deposition;
[0079] The tunnel oxide layer 2 and the intrinsic polysilicon layer 3 are prepared using the same process, which simplifies the preparation process and saves costs;
[0080] S4: preparing barrier layer 4 by low temperature atomic layer deposition;
[0081] Generally, the barrier layer 4 made of aluminum oxide can be prepared by atmospheric pressure chemical vapor deposition, plasma enhanced chemical vapor deposition and low temperature atomic layer deposition. In the present invention, the barrier layer 4 is prepared by low temperature atomic layer deposition to achieve a better thickness control level.
[0082] S5: preparing a doped polysilicon layer 5 by plasma enhanced chemical vapor deposition;
[0083] The doped polysilicon layer 5 and the intrinsic polysilicon layer 3 are prepared by different methods and have different densities. The high-density layer has a better passivation effect and a stronger barrier effect on phosphorus.
[0084] S6: annealing;
[0085] S7: preparing the anti-reflection layer 6 by plasma enhanced chemical vapor deposition.
[0086] It can be understood that in the method for preparing the TOPCON battery 100 provided by the present invention, the intrinsic polysilicon layer 3 and the doped polysilicon layer 5 adopt different manufacturing processes to achieve different densities, thereby improving the passivation effect and enhancing the blocking effect against boron; the barrier layer 4 is prepared by low-temperature atomic layer deposition method, which better realizes the control of the thickness of the barrier layer 4 and further improves the bifaciality of the battery.
[0087] In some optional embodiments, S3: preparing the intrinsic polysilicon layer 3 by low pressure chemical vapor deposition method, comprising the steps of:
[0088] Deposition is started at a first growth temperature for a first time and is increased to a second growth temperature for a second time; the first growth temperature C1, 500°C≤C1≤600°C; the second growth temperature C2, 570°C≤C2≤630°C; the first time T1, 565s≤T1≤965s; the second time T2, 435s≤T2≤935s.
[0089] Optionally, the first growth temperature C1 can be 500℃, 510℃, 520℃, 534℃, 545℃, 550℃, 556℃, 560℃, 565℃, 568℃, 570℃, 578℃, 580℃, 584℃, 588℃, 590℃, 596℃, 598℃ and 600℃; when C1<500℃, the first growth temperature is low, the reaction is not complete, and the quality of the prepared intrinsic polysilicon layer 3 is unstable; when C2>600℃, the first growth temperature is too high, the temperature of the low-temperature stage of the preparation of the intrinsic polysilicon layer 3 is too high, and the density is uneven; therefore, when 500℃≤C1≤600℃, the first growth temperature is of appropriate size, the quality of the small grain stage deposition of the intrinsic polysilicon layer 3 is stable, and the density is balanced.
[0090] Optionally, the second growth temperature C2 can be 570℃, 575℃, 580℃, 585℃, 590℃, 593℃, 600℃, 606℃, 608℃, 610℃, 615℃, 619℃, 620℃, 625℃, 627℃ and 630℃; when C2<570℃, the second growth temperature is too low, and the temperature difference between the high temperature growth stage and the low temperature growth stage of the intrinsic polysilicon layer 3 is small, resulting in a small difference in grain size and uneven density; when C2>630℃, the second growth temperature is too high, and the temperature difference between the high temperature growth stage and the low temperature growth stage of the intrinsic polysilicon layer 3 is too large, which affects the density of the intrinsic polysilicon layer 3.
[0091] Optionally, the first time T1 may be 565s, 575s, 580s, 588s, 590s, 598s, 600s, 635s, 657s, 665s, 670s, 686s, 700s, 725s, 768s, 783s, 790s, 800s, 824s, 836s, 840s, 850s, 856s, 870s, 884s, 890, 900s, 910s, 915s, 920s, 925s, 930s s and 965s, when T1<565s, the low-temperature growth stage time of the intrinsic polysilicon layer 3 is relatively short, which will affect the final density of the intrinsic polysilicon layer 3; when T2>935s, the deposition time of the first growth temperature is too long, and there are too many small grains, which can easily cause the intrinsic polysilicon layer 3 to be uneven; therefore, when 565s≤T1≤965s, the first growth time is appropriate, and the low-temperature growth time of the intrinsic polysilicon layer 3 is appropriate, which is conducive to the growth of the intrinsic polysilicon layer 3 into film layers with different densities and enhances the barrier effect on boron diffusion.
[0092] Optionally, the second time T2 can be 435s, 455s, 467s, 478s, 486s, 490s, 500s, 512s, 524s, 535s, 550s, 560s, 565s, 580s, 590s, 600s, 606s, 620s, 650s, 660s, 680s, 700s, 735s, 760s, 780s, 800s, 830s, 854s, 860s, 874s, 888s, 900s, 915s, 923s and 935s; when T2< When T2 is 435s, the second growth time is short, and the high-temperature growth time of the intrinsic polysilicon layer 3 is short, which affects the density of the intrinsic polysilicon layer 3, and further affects the effect of the intrinsic polysilicon layer 3 in hindering boron diffusion; when T2>935S, the second growth time is too long, which affects the density of the intrinsic polysilicon layer 3, and further affects the effect of the intrinsic polysilicon layer 3 in hindering boron diffusion; therefore, when 435s≤T2≤935s, the second time is appropriate, and the high-temperature growth time of the intrinsic polysilicon layer 3 is appropriate, which is conducive to the growth of the intrinsic polysilicon layer 3 into film layers with different densities and enhances the effect of hindering boron diffusion.
[0093] Optionally, the first growth temperature may be 500°C≤C1≤530°C, 526°C≤C1≤545°C, 530°C≤C1≤560°C, 550°C≤C1≤586°C and 575°C≤C1≤600°C; the second growth temperature C2 may also be 570°C≤C2≤595°C, 580°C≤C2≤605°C, 593°C≤C1≤600°C.
[0094] ≤C2≤616℃, 600℃≤C2≤625℃ and 618℃≤C2≤630℃; the first time T1 can also be 565s≤T1≤665s, 589s≤T1≤690s, 675s≤T1≤800s, 735s≤T1≤865s, 835s≤T1≤935s and 925s≤T1≤965s; the second time T2 can also be 435s≤T2≤589s, 535s≤T2≤735s, 675s≤T2≤855s, 785s≤T2≤903s and 835s≤T2≤935s.
[0095] It should be noted that, S3: when the intrinsic polysilicon layer 3 is prepared by low-pressure chemical vapor deposition, the intrinsic polysilicon layer 3 is divided into small grain growth and large grain growth. The small grains are grown at the first growth temperature for the first time, and the large grains are grown at the second growth temperature for the second time. The density difference is achieved through the grain size, which further hinders the diffusion of boron.
[0096] In some optional embodiments, S4: preparing the barrier layer 4 by low temperature atomic layer deposition method, comprising the steps of:
[0097] The temperature rises to 150℃-225℃;
[0098] Evacuate to a pressure of 0.05-0.3 mTorr;
[0099] A mixed gas of ozone and water vapor and trimethylaluminum are introduced.
[0100] It should be noted that when the temperature is low, the gas reaction activity is poor, the atomic migration rate is low, trimethylaluminum and oxygen-containing active groups are easily cooled by the silicon wafer 1, the nucleation rate is slow or even no nucleation can be formed, which will lead to a rough aluminum oxide surface, poor density, poor field passivation effect, and even the precursor being completely activated or condensed when the temperature is too low; if the temperature is too high, the energy carried by the ions bombarding the surface of the silicon wafer 1 will gradually increase, causing the film-forming part of the aluminum oxide to fall off under the plasma bombardment, aggravating the surface damage of the silicon wafer 1, increasing the recombination of the surface of the silicon wafer 1, and reducing the effective minority carrier lifetime; when the temperature is 150℃-225℃, the atomic mobility is improved, and the atomic nuclei are able to migrate to the appropriate position for nucleation, which is conducive to the overflow of reaction by-products from the surface of the silicon wafer 1, and the prepared barrier layer 4 is flat, dense, and has a good passivation effect.
[0101] It should be noted that the vacuum is evacuated to a pressure of 0.05-0.3 mTorr to form a vacuum constant temperature environment in the process chamber; a mixed gas of ozone and water vapor is introduced to react with trimethylaluminum, and sampling is performed to achieve low-temperature growth. Water vapor achieves a high hydrogen content in the prepared barrier layer 4, providing hydrogen passivation for subsequent annealing. The reaction time is 200s-500s, and the cycle is 1-25 times.
[0102] In some optional embodiments, S2: depositing the tunnel oxide layer 2 by low pressure chemical vapor deposition method, including the conditions: temperature of 550° C.-650° C., time of 350 s-900 s.
[0103] It should be noted that the low-pressure chemical vapor deposition method for depositing the tunnel oxide layer 2 and preparing the intrinsic polysilicon layer 3 can save process steps, can better match the subsequent intrinsic polysilicon layer 3 preparation process, and the quality and uniformity of the grown tunnel oxide layer 2 are better.
[0104] In some optional embodiments, S5: preparing the doped polysilicon layer 5 by plasma enhanced chemical vapor deposition, including the following conditions: the reaction gases are silane and borane, the gas pressure is 70Pa-120Pa, and the temperature is 220°C-400°C.
[0105] It should be noted that the reaction gases are silane and borane, and the ratio of each gas is controlled by a mass flow meter. The range of the doping gas ratio (R = B2H6 / SiH4) is: 1×10 -2 -7.5×10 -4 , a lower borane doping concentration makes it easier for more light to pass through the doped polysilicon layer 5 , thereby improving the performance of the cell 100 .
[0106] In some optional embodiments, S6: annealing, including conditions: temperature of 880° C.-960° C., treatment time of 20 min-40 min.
[0107] It should be noted that the initial solid concentration of doped boron in silicon is low, so high temperature annealing is required. Too high temperature and too long time will cause boron to penetrate the tunneling oxide layer 2, and the Auger load of the silicon wafer 1 will increase; too low temperature or too short time will cause the doping concentration in the doped polysilicon layer 5 to be low, and the long passivation effect of the intrinsic polysilicon layer 3 and the doped polysilicon layer 4 will decrease. Therefore, the annealing effect is better when the temperature is 880℃-960℃ and the treatment is 20min-40min.
[0108] It can be seen from the above embodiments that the TOPCON battery 100 and the preparation method thereof provided by the present invention achieve at least the following beneficial effects:
[0109] The TOPCON cell provided by the present invention comprises a silicon wafer 1 and a tunneling oxide layer 2 arranged on a first surface 11 of the silicon wafer 1 along a first direction y, an intrinsic polysilicon layer 3, a doped polysilicon layer 5 and an anti-reflection layer 6 which are sequentially stacked and arranged on a side of the tunneling oxide layer 2 away from the first surface 11, and a barrier layer 4 is further arranged between the intrinsic polysilicon layer 3 and the doped polysilicon layer 5 along the first direction y, the barrier layer 4 passivates the surface of the intrinsic polysilicon layer 3, realizes hole selective transmission, forms a certain barrier to the subsequent expansion of boron atoms, and reduces the diffusion depth; the barrier layer 4 and the intrinsic polysilicon layer 3 form a multi-layer passivation structure, further enhancing the passivation effect and improving the battery conversion efficiency. efficiency; the thickness of the barrier layer 4 is less than that of the doped polysilicon layer 5, and the thinner barrier layer 4 can achieve a high probability of tunnel effect, further improving the battery conversion efficiency; the setting of the intrinsic polysilicon layer 3 reduces the thickness of the doped polysilicon in the existing battery structure to a certain extent, improves the back efficiency of the TOPCON battery, and improves the bifaciality level; in the preparation method of the TOPCON battery 100 provided by the present invention, the intrinsic polysilicon layer 3 and the doped polysilicon layer 5 adopt different manufacturing processes to achieve different densities, improve the passivation effect, and enhance the blocking effect against boron; the barrier layer 4 is prepared by low-temperature atomic layer deposition method, so as to better realize the control of the thickness of the barrier layer 4.
[0110] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.
Claims
1. A TOPCON battery, characterized in that: include: Silicon wafer; It also includes a tunneling oxide layer disposed on a first surface of the silicon wafer along a first direction, an intrinsic polysilicon layer, a doped polysilicon layer and an anti-reflection layer stacked in sequence on a side of the tunneling oxide layer away from the first surface, the first direction being the thickness direction of the silicon wafer; the first surface being the back side of the battery; Along the first direction, a barrier layer is further provided between the intrinsic polysilicon layer and the doped polysilicon layer, and the thickness of the barrier layer is less than the thickness of the doped polysilicon layer.
2. The TOPCON battery according to claim 1, characterized in that: The silicon wafer is a P-type silicon wafer, and the material of the barrier layer is aluminum oxide; the silicon wafer also includes a second surface, which is the front side of the battery; along the first direction, the second surface is stacked with an N-type emitter, a silicon oxide film and an anti-reflection layer in sequence.
3. The TOPCON battery according to claim 1, characterized in that: Along the first direction, the thickness of the barrier layer is a, 0.1 nm≤a≤1.5 nm.
4. The TOPCON battery according to claim 1, characterized in that: Along the first direction, the thickness c of the tunnel oxide layer is 1.5nm≤c≤3.0nm; the thickness b of the intrinsic polysilicon layer is 40nm≤b≤70nm; and the thickness d of the doped polysilicon layer is 20nm≤d≤50nm.
5. A method for preparing a TOPCON battery, applicable to the TOPCON battery according to any one of claims 1 to 4, characterized in that: Includes steps: Alkali polishing; The tunnel oxide layer is prepared by low pressure chemical vapor deposition method; The intrinsic polysilicon layer is prepared by low pressure chemical vapor deposition method; The barrier layer is prepared by low temperature atomic layer deposition method; The doped polysilicon layer is prepared by plasma enhanced chemical vapor deposition; annealing; The anti-reflection layer is prepared by plasma enhanced chemical vapor deposition.
6. The method for preparing a TOPCON battery according to claim 5, characterized in that: The low pressure chemical vapor deposition method for preparing the intrinsic polysilicon layer comprises the following steps: Deposition is started at a first growth temperature for a first time and the temperature is increased to a second growth temperature for a second time; The first growth temperature C1, 500°C≤C1≤600°C; the second growth temperature C2, 570°C≤C2≤630°C; the first time T1, 565s≤T1≤965s; the second time T2, 435s≤T2≤935s.
7. The method for preparing a TOPCON battery according to claim 5, characterized in that: The low temperature atomic layer deposition method for preparing the barrier layer comprises the following steps: The temperature rises to 150℃-225℃; Evacuate to a pressure of 0.05-0.3 mTorr; A mixed gas of ozone and water vapor and trimethylaluminum are introduced.
8. The method for preparing a TOPCON battery according to claim 5, characterized in that: The tunnel oxide layer is deposited by the low pressure chemical vapor deposition method, including the following conditions: temperature of 550° C.-650° C. and time of 350s-900s.
9. The method for preparing a TOPCON battery according to claim 5, characterized in that: The plasma enhanced chemical vapor deposition method for preparing the doped polysilicon layer includes the following conditions: the reaction gases are silane and borane, the gas pressure is 70Pa-120Pa, and the temperature is 220°C-400°C.
10. The method for preparing a TOPCON battery according to claim 5, characterized in that: The annealing includes the following conditions: temperature is 880° C.-960° C., and the treatment time is 20 min-40 min.
Citation Information
Cited By
Passivating film layer structure, preparation method thereof and application of passivating film layer structure in preparation of solar cell
CN120769614A
Battery emitting electrode composite film layer structure, preparation method thereof and application of battery emitting electrode composite film layer structure in preparation of solar battery
CN120813125A