Battery negative plate, preparation method thereof and lithium ion battery
By using a multi-layer structure of modified porous alumina and negative electrode active substances in lithium batteries, the power attenuation problem of traditional lithium batteries during high power output is solved, the dynamic performance and safety of the battery are improved, and the fast charging is met and high energy demand.
Patent Information
- Application Number
- CN202411039455.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional lithium batteries are prone to power attenuation when output at high power, and even cause the battery to overheat or fail, which cannot meet the needs of fast charging and high energy.
Modified porous alumina is used as the material for the negative electrode sheet of the battery, and the multi-layer coating structure is formed by mixing the porous alumina modified by 3-aminopropyltriethoxysilane with the negative electrode active material, conductive agent and binder. , to improve the liquid absorption rate of electrolyte and the migration ability of lithium ions, enhance the conductivity and breathability of electrons, and reduce internal resistance.
It improves the dynamic performance and rate performance of lithium-ion batteries, optimizes safety, meets the needs of high-power applications, and extends the service life of the battery.
Smart Images

Figure CN118983399A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium batteries, and in particular relates to a battery negative electrode sheet and a preparation method thereof and a lithium ion battery. Background Art
[0002] Consumers are increasingly demanding faster charging speeds for electronic products and electric vehicles, and this has led to higher demands for the fast charging capabilities of lithium-ion batteries as energy carriers. Although traditional lithium batteries have high energy density, their power output capacity is low. When the demand exceeds the discharge rate of the standard capacity, traditional lithium batteries are prone to power attenuation, and may even cause the battery to overheat, be damaged, or fail. Therefore, the present invention is derived from this. Summary of the invention
[0003] In view of one of the above-mentioned technical problems, the object of the present invention is to provide a battery negative electrode sheet and a preparation method thereof and a lithium ion battery.
[0004] The technical solution of the present invention is:
[0005] One of the objects of the present invention is to provide a method for preparing a negative electrode sheet of a battery, comprising the following steps:
[0006] Mixing a negative electrode active material, a first binder, a conductive agent, a suspension of modified porous alumina and a solvent to obtain a negative electrode slurry; coating the obtained negative electrode slurry on at least one surface of a negative electrode current collector to obtain a negative electrode active material coating;
[0007] Among them, the modified porous alumina is porous alumina modified with 3-aminopropyltriethoxysilane and its weight ratio in the negative electrode slurry is 3%-10%, and the negative electrode active material, modified porous alumina, first binder and conductive agent are in a mass ratio of (85-94):(2-10):(2-3.5):(1-3).
[0008] Another method for preparing a negative electrode sheet of a battery provided by the present invention comprises coating a first negative electrode slurry containing no modified porous alumina and a negative electrode active material on at least one surface of a negative electrode current collector to obtain a first negative electrode coating, and then coating a second negative electrode slurry containing modified porous alumina and no negative electrode active material on the surface of the first negative electrode coating to form a second negative electrode coating;
[0009] Wherein, the modified porous alumina is a porous alumina modified with 3-aminopropyltriethoxysilane and its weight ratio in the second negative electrode slurry is 40%-70%, the first negative electrode slurry comprises a negative electrode active material, a first binder, a conductive agent and a solvent and the negative electrode active material, the first binder and the conductive agent are in a mass ratio of (90-97):(2-3.5):(1-3), the second negative electrode slurry comprises modified porous alumina, a second binder, a conductive agent and a solvent and the modified porous alumina, the second binder and the conductive agent are in a mass ratio of (85-97):(2-10):(1-5), and the second binder is polyvinylidene fluoride.
[0010] Another method for preparing a negative electrode sheet of a battery provided by the present invention comprises the following steps:
[0011] Applying a second negative electrode slurry containing modified porous alumina and not containing negative electrode active material on at least one surface of the negative electrode current collector to obtain a second negative electrode coating, and then applying a first negative electrode slurry containing no modified porous alumina and containing negative electrode active material on the surface of the second negative electrode coating to form a first negative electrode coating;
[0012] Wherein, the modified porous alumina is a porous alumina modified with 3-aminopropyltriethoxysilane and its weight ratio in the second negative electrode slurry is 40%-70%, the first negative electrode slurry comprises a negative electrode active material, a first binder, a conductive agent and a solvent and the negative electrode active material, the first binder and the conductive agent are in a mass ratio of (90-97):(2-3.5):(1-3), the second negative electrode slurry comprises modified porous alumina, a second binder, a conductive agent and a solvent and the modified porous alumina, the second binder and the conductive agent are in a mass ratio of (85-97):(2-10):(1-5), and the second binder is polyvinylidene fluoride.
[0013] Another method for preparing a negative electrode sheet of a battery provided by the present invention comprises the following steps:
[0014] A first negative electrode active material, a first binder, a conductive agent, a suspension of modified porous alumina and a solvent are mixed to obtain a negative electrode slurry 1; the prepared negative electrode slurry 1 is coated on at least one surface of a negative electrode current collector to obtain a first negative electrode active material coating;
[0015] The second negative electrode active material, the first binder, the conductive agent, the suspension of modified porous alumina and the solvent are mixed to obtain a negative electrode slurry 2; the obtained negative electrode slurry 2 is coated on the surface of the first negative electrode active material coating to obtain a second negative electrode active material coating;
[0016] Wherein, the modified porous alumina is porous alumina modified by 3-aminopropyltriethoxysilane and the weight ratio of the modified porous alumina in the negative electrode slurry is 3%-10%;
[0017] The first negative electrode active material and the second negative electrode active material are both graphite, and the second negative electrode active material is artificial graphite that has been subjected to carbon coating treatment, and the first negative electrode active material is artificial graphite that has not been subjected to carbon coating treatment.
[0018] Preferably, the negative electrode active material comprises at least one of graphite, silicon oxide, and silicon carbon, wherein the graphite is carbon-coated artificial graphite or a mixture of carbon-coated artificial graphite and uncoated artificial graphite, wherein the graphite, silicon oxide, and silicon carbon are in the following weight percentages: graphite: 70-100%, silicon oxide: 0-20%, silicon carbon: 0-20%; and / or
[0019] The conductive agent is conductive carbon black and / or carbon nanotubes; and / or
[0020] The first binder is any one or two of styrene-butadiene rubber latex, sodium carboxymethyl cellulose, and polyacrylic acid; and / or
[0021] The solvent is N-methylpyrrolidone or water.
[0022] Preferably, the method for preparing the porous alumina modified with 3-aminopropyltriethoxysilane comprises the following steps:
[0023] 3-aminopropyltriethoxysilane and ethanol are mixed in a volume ratio of 1:4 to obtain a mixed solution, and the porous alumina and the mixed solution are evenly mixed in a mass ratio of 3-aminopropyltriethoxysilane to porous alumina of 2:8. After reacting for 2 hours under an ultrasonic vibration environment, the mixture is placed in a vacuum drying oven and dried at 60°C for 24-48 hours to obtain the 3-aminopropyltriethoxysilane-modified porous alumina.
[0024] Preferably, the particle size of the porous alumina modified by 3-aminopropyltriethoxysilane is D10: 0.15-0.25 μm, D50: 0.42-0.6 μm, D90: 1.8-2.2 μm, and the specific surface area is 16-24 m 2 / g, pore size is 6-12nm.
[0025] Preferably, the coating density of the coating containing the negative electrode active material is 6-12 mg / cm 2 The surface density of the coating containing only modified porous alumina and no negative electrode active material is 1.0-3.0 mg / cm 2 .
[0026] Another object of the present invention is to provide a battery negative electrode sheet, comprising a negative electrode current collector and a coating coated on at least one side of the negative electrode current collector, wherein the coating is a coating containing a negative electrode active material in any of the above items and a coating containing only modified porous alumina but no negative electrode active material, and the negative electrode sheet is prepared by the preparation method described in any of the above items.
[0027] Another object of the present invention is to provide a lithium-ion battery, comprising a negative electrode sheet prepared by any of the preparation methods described above or comprising the battery negative electrode sheet described above.
[0028] Compared with the prior art, the advantages of the present invention are:
[0029] The present invention obtains modified porous alumina by modifying porous alumina powder, and applies it to the negative electrode sheet of the battery. The porous morphology of the modified alumina can be more conducive to improving the liquid absorption rate of the electrolyte, increasing the channel of the electrolyte, facilitating the migration of lithium ions, improving the dynamic performance of the battery, and improving the electronic conductivity of the negative electrode sheet material. At the same time, the porous morphology can greatly increase the air permeability and porosity, thereby reducing the internal resistance, improving the rate performance, and optimizing the safety. On the one hand, by optimizing the ratio of the modified porous alumina in the negative electrode slurry, on the other hand, by optimizing the electrode material and structure of the electrode sheet, the problem of low power output capacity of the existing traditional lithium battery is improved to meet the needs of high-power applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0031] Figure 1 It is a schematic diagram of the structure of the negative electrode sheet of the battery of Examples 1 to 4 of the present invention and Comparative Example 1;
[0032] Figure 2 It is a comparative curve diagram of rate discharge of batteries including the negative electrode sheets of Examples 1 to 4 of the present invention and Comparative Example 1;
[0033] Figure 3 It is a comparative curve diagram of the charging rate of the battery including the negative electrode sheets of Examples 1 to 4 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0035] An embodiment of the present invention provides a method for preparing a negative electrode sheet of a battery, comprising the following steps:
[0036] A negative electrode slurry is prepared by mixing a negative electrode active material, a first binder, a conductive agent, a suspension of modified porous alumina, and a solvent; the prepared negative electrode slurry is coated on at least one surface (preferably two surfaces) of a negative electrode current collector to obtain a negative electrode active material coating (i.e., a coating containing a negative electrode active material);
[0037] Among them, the modified porous alumina is porous alumina modified with 3-aminopropyltriethoxysilane and its weight ratio in the negative electrode slurry is 3%-10%, and the negative electrode active material, modified porous alumina, first binder and conductive agent are in a mass ratio of (85-94):(2-10):(2-3.5):(1-3).
[0038] In the above embodiment, the negative electrode active material is directly mixed with modified porous alumina, a conductive agent, a binder and a solvent to obtain a slurry, which is then coated on the two surfaces of the negative electrode collector to obtain a battery negative electrode sheet. That is, the battery negative electrode sheet prepared by the preparation method of the above embodiment includes a negative electrode collector and a coating coated on the two surfaces of the negative electrode collector (the coating is a coating containing a negative electrode active material).
[0039] As a variation of the above embodiment, the embodiment of the present invention provides a method for preparing a negative electrode sheet of a battery, wherein a suspension containing a negative electrode active material, a first binder, a conductive agent, and a modified porous alumina is mixed with a solvent to prepare two negative electrode slurries respectively, the main difference being that the negative electrode active materials in the two negative electrode slurries are different, and the two negative electrode slurries are successively coated on the two surfaces of the negative electrode current collector to obtain a negative electrode sheet. Specifically, the method comprises the following steps:
[0040] A first negative electrode active material, a first binder, a conductive agent, a suspension of modified porous alumina and a solvent are mixed to obtain a negative electrode slurry 1; the obtained negative electrode slurry 1 is coated on at least one surface, preferably two surfaces, of a negative electrode current collector to obtain a first negative electrode active material coating (i.e., a coating containing a negative electrode active material);
[0041] The second negative electrode active material, the first binder, the conductive agent, the suspension of modified porous alumina and the solvent are mixed to obtain a negative electrode slurry 2; the obtained negative electrode slurry 2 is coated on the surface of the first negative electrode active material coating to obtain a second negative electrode active material coating (i.e., a coating containing the negative electrode active material);
[0042] Wherein, the modified porous alumina is porous alumina modified by 3-aminopropyltriethoxysilane and its weight ratio in the negative electrode slurry is 3%-10%;
[0043] The first negative electrode active material and the second negative electrode active material are both graphite. More specifically, the second negative electrode active material is carbon-coated artificial graphite, and the first negative electrode active material is uncoated artificial graphite.
[0044] That is, the battery negative electrode sheet prepared by the preparation method of the above embodiment includes a negative electrode current collector and a first negative electrode active material coating and a second negative electrode active material coating respectively coated on two surfaces of the negative electrode current collector, both coatings are coatings containing active materials, and the active material of the inner coating is graphite without carbon coating, and the active material of the outer coating is graphite coated with carbon. The mechanical strength of the battery negative electrode sheet can be effectively improved.
[0045] Another embodiment of the present invention provides another method for preparing a negative electrode sheet of a battery, comprising the following steps:
[0046] Coating a first negative electrode slurry containing no modified porous alumina and containing a negative electrode active material on at least one surface of a negative electrode current collector to obtain a first negative electrode coating (i.e., a coating containing a negative electrode active material), and then coating a second negative electrode slurry containing modified porous alumina and containing no negative electrode active material on the surface of the first negative electrode coating to form a second negative electrode coating (i.e., a coating containing only modified porous alumina and containing no negative electrode active material);
[0047] Among them, the modified porous alumina is 3-aminopropyltriethoxysilane modified porous alumina and its weight ratio in the second negative electrode slurry is 40%-70%, the first negative electrode slurry includes a negative electrode active material, a first binder, a conductive agent and a solvent, and the negative electrode active material, the first binder and the conductive agent are in a mass ratio of (90-97):(2-3.5):(1-3), the second negative electrode slurry includes modified porous alumina, a second binder, a conductive agent and a solvent, and the modified porous alumina, the second binder and the conductive agent are in a mass ratio of (85-97):(2-10):(1-5), and the second binder is polyvinylidene fluoride.
[0048] That is, the battery negative electrode sheet prepared by the preparation method of the above embodiment includes a negative electrode current collector and a first negative electrode coating and a second negative electrode coating respectively coated on the two surfaces of the negative electrode current collector, the first negative electrode coating is located on the inner side of the second negative electrode coating, and the first negative electrode coating is a coating containing a negative electrode active substance, and the second negative electrode coating is a coating containing modified porous alumina but not containing a negative electrode active substance.
[0049] As a variation of the above-mentioned method for preparing another negative electrode sheet of a battery, another embodiment of the present invention provides another method for preparing a negative electrode sheet of a battery, comprising the following steps:
[0050] The second negative electrode slurry containing modified porous alumina and not containing negative electrode active material is coated on at least one surface, preferably two surfaces, of the negative electrode current collector to obtain a second negative electrode coating (i.e., a coating containing only modified porous alumina and not containing negative electrode active material), and the first negative electrode slurry containing no modified porous alumina and containing negative electrode active material is coated on the surface of the second negative electrode coating to form a first negative electrode coating (i.e., a coating containing negative electrode active material);
[0051] Among them, the modified porous alumina is 3-aminopropyltriethoxysilane modified porous alumina and its weight ratio in the second negative electrode slurry is 40%-70%, the first negative electrode slurry includes a negative electrode active material, a first binder, a conductive agent and a solvent, and the negative electrode active material, the first binder and the conductive agent are in a mass ratio of (90-97):(2-3.5):(1-3), the second negative electrode slurry includes modified porous alumina, a second binder, a conductive agent and a solvent, and the modified porous alumina, the second binder and the conductive agent are in a mass ratio of (85-97):(2-10):(1-5), and the second binder is polyvinylidene fluoride.
[0052] That is, the battery negative electrode sheet prepared by the preparation method of the above embodiment includes a negative electrode current collector and a first negative electrode coating and a second negative electrode coating respectively coated on the two surfaces of the negative electrode current collector, the first negative electrode coating is located on the outside of the second negative electrode coating, and the first negative electrode coating is a coating containing a negative electrode active substance, and the second negative electrode coating is a coating containing modified porous alumina but not containing a negative electrode active substance.
[0053] It should be noted that the coatings in the above embodiments are mainly divided into two categories, one is a coating containing negative electrode active materials, and the other is a coating containing only modified porous alumina but no negative electrode active materials. Preferably, the coating surface density of the coating containing negative electrode active materials is 6-12 mg / cm per side. 2 The surface density of the coating containing only modified porous alumina and no negative electrode active material is 1.0-3.0 mg / cm 2 .
[0054] In the above embodiments, except for the first variant embodiment, the negative electrode active material in the remaining embodiments includes at least one of graphite, silicon oxide, and silicon carbon (that is, it can be any one of them, it can be a mixture of any two, or it can be a mixture of three), and the graphite is carbon-coated artificial graphite or a mixture of carbon-coated artificial graphite and uncoated artificial graphite, wherein the graphite, silicon oxide and silicon carbon are in the following weight percentages: graphite: 70-100%, silicon oxide: 0-20%, silicon carbon: 0-20%. It should be noted that the above silicon oxide is silicon monoxide, which can be represented by the chemical formula SiOx, where 0<x≤2, and can be purchased commercially. The above silicon carbon is a carbon-coated silicon material available on the market. The method of carbon coating treatment can be selected from those familiar to those skilled in the art, such as chemical vapor deposition, physical vapor deposition, solution method, etc., without specific description and limitation. Silicon has a high theoretical specific capacity and specific energy density, and can achieve a higher ability to embed and deintercalate lithium ions. However, embedding causes volume expansion, and deintercalation causes volume contraction. In the embodiments of the present invention, the composition and ratio of the components are reasonably designed to meet the balance of conductivity, stability and performance.
[0055] In the above embodiment, the conductive agent is conductive carbon black and / or carbon nanotubes. In the above embodiment, the first binder is any one or two of styrene-butadiene rubber latex, sodium carboxymethyl cellulose, and polyacrylic acid. In the above embodiment, the solvent is N-methyl pyrrolidone or water.
[0056] In the above embodiment, the modified porous alumina is a porous alumina modified with 3-aminopropyltriethoxysilane. The properties of the raw porous alumina used in the modified porous alumina and the preparation method are all referenced to the porous needle-shaped alumina powder described in the Chinese patent document CN117416981A. Specifically, the preparation method of the porous alumina modified with 3-aminopropyltriethoxysilane is as follows: 3-aminopropyltriethoxysilane and ethanol are mixed in a volume ratio of 1:4 to obtain a mixed solution, and the porous alumina and the mixed solution are evenly mixed in a mass ratio of 3-aminopropyltriethoxysilane to porous alumina of 2:8, and reacted under an ultrasonic vibration environment for 2 hours, and then placed in a vacuum drying oven, and dried at 60°C for 24-48 hours to obtain 3-aminopropyltriethoxysilane-modified porous alumina (for ease of description, the subsequent use of Si-N-Al 2 O 3 Its structural formula is as follows: Wherein R represents the porous needle-shaped alumina powder (Al 2 O 3 ), and in the formula It means that -O- forms the same structural formula with other Si and alumina, so this symbol is used here instead. For details, please refer to Section 2.1.3.1 of Chapter 2 of the thesis (Liao Yiming. Preparation of inorganic nanomaterials modified with aminopropyltriethoxysilane and research on its effect on the tracking resistance of silicone rubber [D]. Guangzhou: South China University of Technology, 2022.). In addition, the above-mentioned 3-aminopropyltriethoxysilane is a conventional product currently sold on the market, and is not specifically limited. The modified porous alumina in the embodiment of the present invention has the following properties: The particle size of the porous alumina modified with 3-aminopropyltriethoxysilane is D10: 0.15~0.25μm, D50: 0.42~0.6μm, D90: 1.8~2.2μm, and the specific surface area is 16~24m 2 / g, pore size is 6-12nm.
[0057] In the above embodiments, the negative electrode current collector is selected from one or more of copper foil, carbon-coated copper foil, and perforated copper foil.
[0058] In the embodiment of the present invention, modified porous alumina is added as an additive to the coating slurry of the negative electrode sheet to increase the transmission channel of the electrolyte, improve the kinetic performance of the battery and the electronic conductivity of the material, and improve the rate performance; the surface of the porous alumina is modified by 3-aminopropyltriethoxysilane to increase the adhesion between the inorganic particle porous alumina and the negative electrode current collector.
[0059] The various chemical reagents and substances mentioned in the above embodiments are all directly available on the market and are not specifically described or limited.
[0060] Another aspect of the present invention is to provide a negative electrode sheet for a battery manufactured by the manufacturing method of the above embodiment.
[0061] Another aspect of the embodiments of the present invention provides a lithium-ion battery including the battery negative electrode sheet of the above embodiment.
[0062] Specifically, the preparation and physical properties of lithium-ion batteries:
[0063] Lithium nickel cobalt manganese oxide, polyvinylidene fluoride (PVDF), and conductive carbon black (Super P) were mixed in a mass ratio of 96:2:2, and N-methylpyrrolidone (NMP) was added and stirred under the action of a double planetary mixer until a uniform positive electrode slurry was mixed. The positive electrode slurry was evenly coated on an aluminum foil with a thickness of 12 μm by an extrusion coater, and then dried, rolled, and then cut to obtain the required positive electrode sheet.
[0064] The positive electrode sheet, the separator and the negative electrode sheet prepared in the above embodiment are stacked in order to ensure that the separator is between the positive and negative electrode sheets to play an isolating role, and then the bare battery cell without liquid injection is obtained by winding. The bare battery cell is placed in an aluminum-plastic film shell, and the prepared electrolyte is injected into the dried bare battery cell. After vacuum packaging, standing, forming, shaping, sorting and other processes, the desired lithium-ion battery is obtained. The specific process parameters are not described and limited. It is an existing conventional method for preparing lithium-ion batteries, which is easy for those skilled in the art to know and implement, and is not the innovation of the present invention.
[0065] According to the test, the lithium-ion battery of the embodiment of the present invention can meet the stable cycle under the conditions of 8-10C charging and 8-15C discharging.
[0066] The embodiment of the present invention optimizes the porous alumina modification process and the ratio of the modified porous alumina to the negative electrode slurry, and optimizes the structure and electrode material in the negative electrode sheet, so that the prepared negative electrode sheet can be applied to lithium batteries to meet high-power applications.
[0067] Example 1
[0068] Graphite, sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber (SBR), and conductive carbon black were mixed in a mass ratio of 96.5:1.2:1.5:0.8, and deionized water was added (the weight ratio of deionized water to the above substances was 2:3, ensuring that the solid content in the entire solution was about 60%), and the first negative electrode slurry was obtained under the action of a double planetary mixer. 2 O 3 , PVDF, and conductive carbon black are mixed in a mass ratio of 96:1.2:1.5, and NMP is added (same as above, the weight ratio of NMP to the above substances is 2:3, ensuring that the solid content in the whole solution is about 60%), and the second negative electrode slurry is obtained under the action of a double planetary mixer. The first negative electrode slurry is applied on a copper foil by an extrusion coater, and after drying, a first negative electrode coating, i.e., a negative electrode active material layer, is obtained. The second negative electrode slurry is applied on the first negative electrode coating, i.e., the negative electrode active material layer, to form a second negative electrode coating, and after drying, the negative electrode sheet is obtained by rolling and slitting.
[0069] Example 2
[0070] Graphite, Si-N-Al 2 O 3, sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber (SBR), and conductive carbon black are mixed in a mass ratio of 90.5:6:1.2:1.5:0.8, and deionized water is added (the weight ratio of deionized water to the above substances is 2:3, ensuring that the solid content in the entire solution is about 60%), and the negative electrode slurry is obtained under the action of a double planetary mixer. The negative electrode slurry is coated on a copper foil (negative electrode current collector) by an extrusion coater, and after drying, it is rolled and cut to obtain a negative electrode sheet.
[0071] Example 3
[0072] Graphite 1 (i.e., the first negative electrode active material, in the embodiment of the present invention, graphite 1 is uncoated artificial graphite), Si-N-Al 2 O 3 , sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber (SBR), and conductive carbon black are mixed in a mass ratio of 96.5:6:1.2:1.5:0.8, and deionized water is added (the weight ratio of deionized water to the above substances is 2:3, ensuring that the solid content in the entire solution is about 60%), and negative electrode slurry 1 is obtained under the action of a double planetary mixer. Graphite 2 (i.e., the second negative electrode active material, in the embodiment of the present invention, graphite 2 is artificial graphite coated with asphalt, and asphalt is a soft carbon) and Si-N-Al 2 O 3 , sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber (SBR), and carbon black were mixed in a mass ratio of 90.5:6:1.2:1.5:0.8, and NMP was added (the weight ratio of NMP to the above substances was 2:3, ensuring that the solid content in the entire solution was about 60%), and negative electrode slurry 2 was obtained under the action of a double planetary mixer. The negative electrode slurry 1 was applied on a copper foil by an extrusion coater, and the first negative electrode active material layer was obtained after drying. The negative electrode slurry 2 was applied on the first negative electrode active material layer to form a second negative electrode active material layer, and the negative electrode sheet was obtained after drying, rolling, and slitting.
[0073] Example 4
[0074] Si-N-Al 2 O 3, PVDF, and conductive carbon black are mixed in a mass ratio of 96:1.2:1.5, and NMP is added (the weight ratio of NMP to the above substances is 2:3, ensuring that the solid content in the whole solution is about 60%), and the second negative electrode slurry is obtained under the action of a double planetary mixer. The second negative electrode slurry is coated on the copper foil with a coating machine to obtain the second negative electrode coating. Graphite, sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber (SBR), and conductive carbon black are mixed in a mass ratio of 96.5:1.2:1.5:0.8, and deionized water is added (the weight ratio of deionized water to the above substances is 2:3, ensuring that the solid content in the whole solution is about 60%), and the first negative electrode slurry is obtained under the action of a double planetary mixer. The first negative electrode slurry is applied to the surface of the copper foil coated with the second negative electrode coating to form the first negative electrode coating, and after drying, the negative electrode sheet is obtained by rolling and slitting.
[0075] Comparative Example 1
[0076] Graphite, sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber (SBR), and conductive carbon black are mixed in a mass ratio of 96.8:1.2:1.5:1.5, and deionized water is added (the weight ratio of deionized water to the above substances is 2:3, ensuring that the solid content of the entire solution is about 60%), and the negative electrode slurry is obtained under the action of a double planetary mixer. The negative electrode slurry is applied to copper foil with an extrusion coater, and after drying, it is rolled and cut to obtain a negative electrode sheet.
[0077] The applicant has obtained the structure diagram of the negative electrode sheet by the method of Example 1 to Example 4 and Comparative Example 1, specifically, as shown in FIG. Figure 1 As shown, (a) to (d) in the figure correspond to Examples 1 to 4 respectively, and (e) in the figure corresponds to Comparative Example 1. The solid squares at the bottom of Figures (a) to (e) represent the current collector. It can be seen from the figure that in Figure (a), that is, the negative electrode sheet of Example 1, the porous ceramic is on the electrode sheet and there is no active material in the upper layer. In Figure (b), that is, the negative electrode sheet of Example 2, the porous ceramic is evenly distributed in each layer. In Figure (c), that is, the negative electrode sheet of Example 3, the porous ceramic is evenly distributed in each layer and there are active materials in the upper and lower layers, and the active materials in the upper and lower layers are different. In Figure (d), that is, the negative electrode sheet of Example 4, the porous ceramic is in the lower layer of the electrode sheet and there are active materials in the upper and lower layers. In Figure (e), that is, no porous ceramic is found in the negative electrode sheet of Comparative Example 1. It should be noted that in the above description, the lower layer of the electrode sheet is a layer close to the current collector, and the upper layer is a layer away from the current collector.
[0078] Depend on Figure 2 The rate discharge curves of the batteries including the negative electrode sheets of Examples 1 to 4 of the present invention and Comparative Example 1 show that, under the same battery system, the modified porous alumina (Si-N-Al 2 O 3) has a higher capacity than the negative electrode sheet without the modified porous alumina according to the embodiment of the present invention, that is, comparative example 1, and especially the capacity of embodiment 3 with two layers of different negative electrode active materials is the highest.
[0079] Depend on Figure 3 From the rate charging curves of the batteries comprising the negative electrode sheets of Examples 1 to 4 of the present invention and Comparative Example 1, it can be seen that the charging capacity of the negative electrode sheets comprising the modified alumina of the embodiments of the present invention is obviously higher than the charging capacity of the negative electrode sheets not containing modified alumina, i.e., the negative electrode sheets of Comparative Example 1.
[0080] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a negative electrode sheet of a battery, It is characterized in that The following steps are involved: Mixing a negative electrode active material, a first binder, a conductive agent, a suspension of modified porous alumina and a solvent to obtain a negative electrode slurry; coating the obtained negative electrode slurry on at least one surface of a negative electrode current collector to obtain a negative electrode active material coating; Among them, the modified porous alumina is porous alumina modified with 3-aminopropyltriethoxysilane and its weight ratio in the negative electrode slurry is 3%-10%, and the negative electrode active material, modified porous alumina, first binder and conductive agent are in a mass ratio of (85-94):(2-10):(2-3.5):(1-3).
2. A method for preparing a negative electrode sheet of a battery, It is characterized in that Coating a first negative electrode slurry containing no modified porous alumina and containing a negative electrode active material on at least one surface of a negative electrode current collector to obtain a first negative electrode coating, and then coating a second negative electrode slurry containing modified porous alumina and containing no negative electrode active material on the surface of the first negative electrode coating to form a second negative electrode coating; Wherein, the modified porous alumina is a porous alumina modified with 3-aminopropyltriethoxysilane and its weight ratio in the second negative electrode slurry is 40%-70%, the first negative electrode slurry comprises a negative electrode active material, a first binder, a conductive agent and a solvent and the negative electrode active material, the first binder and the conductive agent are in a mass ratio of (90-97):(2-3.5):(1-3), the second negative electrode slurry comprises modified porous alumina, a second binder, a conductive agent and a solvent and the modified porous alumina, the second binder and the conductive agent are in a mass ratio of (85-97):(2-10):(1-5), and the second binder is polyvinylidene fluoride.
3. A method for preparing a negative electrode sheet of a battery, It is characterized in that The following steps are involved: Applying a second negative electrode slurry containing modified porous alumina and not containing negative electrode active material on at least one surface of the negative electrode current collector to obtain a second negative electrode coating, and then applying a first negative electrode slurry containing no modified porous alumina and containing negative electrode active material on the surface of the second negative electrode coating to form a first negative electrode coating; Wherein, the modified porous alumina is a porous alumina modified with 3-aminopropyltriethoxysilane and its weight ratio in the second negative electrode slurry is 40%-70%, the first negative electrode slurry comprises a negative electrode active material, a first binder, a conductive agent and a solvent and the negative electrode active material, the first binder and the conductive agent are in a mass ratio of (90-97):(2-3.5):(1-3), the second negative electrode slurry comprises modified porous alumina, a second binder, a conductive agent and a solvent and the modified porous alumina, the second binder and the conductive agent are in a mass ratio of (85-97):(2-10):(1-5), and the second binder is polyvinylidene fluoride.
4. A method for preparing a negative electrode sheet of a battery, It is characterized in that The following steps are involved: A first negative electrode active material, a first binder, a conductive agent, a suspension of modified porous alumina and a solvent are mixed to obtain a negative electrode slurry 1; the prepared negative electrode slurry 1 is coated on at least one surface of a negative electrode current collector to obtain a first negative electrode active material coating; The second negative electrode active material, the first binder, the conductive agent, the suspension of modified porous alumina and the solvent are mixed to obtain a negative electrode slurry 2; the obtained negative electrode slurry 2 is coated on the surface of the first negative electrode active material coating to obtain a second negative electrode active material coating; Wherein, the modified porous alumina is porous alumina modified by 3-aminopropyltriethoxysilane and the weight ratio in the negative electrode slurry is 3%-10%; The first negative electrode active material and the second negative electrode active material are both graphite, and the second negative electrode active material is artificial graphite that has been subjected to carbon coating treatment, and the first negative electrode active material is artificial graphite that has not been subjected to carbon coating treatment.
5. The preparation method according to any one of claims 1 to 4, It is characterized in that The negative electrode active material comprises at least one of graphite, silicon oxide, and silicon carbon, wherein the graphite is carbon-coated artificial graphite or a mixture of carbon-coated artificial graphite and uncoated artificial graphite, wherein the graphite, silicon oxide, and silicon carbon are in the following weight percentages: graphite: 70-100%, silicon oxide: 0-20%, silicon carbon: 0-20%; and / or The conductive agent is conductive carbon black and / or carbon nanotubes; and / or The first binder is any one or two of styrene-butadiene rubber latex, sodium carboxymethyl cellulose, and polyacrylic acid; and / or The solvent is N-methylpyrrolidone or water.
6. The preparation method according to any one of claims 1 to 4, It is characterized in that The preparation method of the porous alumina modified by 3-aminopropyltriethoxysilane comprises the following steps: 3-aminopropyltriethoxysilane and ethanol are mixed in a volume ratio of 1:4 to obtain a mixed solution, and the porous alumina and the mixed solution are evenly mixed in a mass ratio of 3-aminopropyltriethoxysilane to porous alumina of 2:
8. After reacting for 2 hours under an ultrasonic vibration environment, the mixture is placed in a vacuum drying oven and dried at 60°C for 24-48 hours to obtain the 3-aminopropyltriethoxysilane-modified porous alumina.
7. The preparation method according to claim 6, It is characterized in that The particle size of the porous alumina modified by 3-aminopropyltriethoxysilane is D10: 0.15-0.25 μm, D50: 0.42-0.6 μm, D90: 1.8-2.2 μm, and the specific surface area is 16-24 m 2 / g, pore size is 6-12nm.
8. The preparation method according to any one of claims 1 to 7, It is characterized in that The coating density of the coating containing the negative electrode active material is 6-12 mg / cm per side. 2 The surface density of the coating containing only modified porous alumina and no negative electrode active material is 1.0-3.0 mg / cm 2 .
9. A battery negative electrode sheet, comprising a negative electrode current collector and a coating coated on at least one side of the negative electrode current collector, It is characterized in that The coating is a coating containing negative electrode active material in any one of claims 1-8 and a coating containing only modified porous alumina but no negative electrode active material, and the negative electrode sheet is prepared by the preparation method described in any one of claims 1-8.
10. A lithium ion battery, It is characterized in that A negative electrode sheet prepared by the preparation method according to any one of claims 1 to 8 or a battery negative electrode sheet according to claim 9.
Citation Information
Cited By
Modified graphite negative electrode material and preparation method thereof, negative electrode and lithium ion battery
CN122000333A