Polarization resistance separation method suitable for large-area anode support type SOFC

Through polarization curve testing and Newton's iterative method fitting, the problem of polarization resistance diagnosis in large-area SOFC was solved, and the accurate identification and analysis of polarization resistance was achieved, which improved the power generation performance and durability of SOFC.

CN118983477APending Publication Date: 2024-11-19TIANJIN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040028.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art is difficult to accurately diagnose polarization resistance in large-area solid oxide fuel cells (SOFCs), especially under high temperature environments and complex anode fuel composition, which makes it difficult to effectively monitor and analyze battery performance attenuation.

Method used

By using the polarization curve test method, the relationship between the voltage and current density of SOFC is established and fitted with the Newton iterative method, each polarization resistance is separated, and the influence of gas concentration distribution and electron conductance is accurately identified under different current density. the polarization resistance changes.

Benefits of technology

Accurate identification and analysis of polarization resistance of large-area SOFCs is achieved, providing guidance on improving power generation performance and durability, and being able to evaluate the performance of battery cells and electrolyte membranes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983477A_ABST
    Figure CN118983477A_ABST
Patent Text Reader

Abstract

The invention discloses a polarization resistance separation method suitable for a large-area anode-supported SOFC (Solid Oxide Fuel Cell), which comprises the following steps: controlling the temperature of the activated SOFC at an operating temperature, respectively introducing air and fuel with a certain volume flow into a cathode and an anode, preheating the introduced gas to the operating temperature of the SOFC, and carrying out a polarization curve test; establishing a relational expression of voltage and current of the SOFC lumped; dividing regions according to the magnitude of the current density, establishing a polarization resistance separation model, fitting a relational expression of the voltage and the current density of the SOFC lumped with a polarization curve test result, and obtaining each electrochemical parameter according to a fitting result; and obtaining gas concentration resistance and cathode charge transfer resistance based on the obtained electrochemical parameters. The model algorithm is simple and effective, various types of polarization resistance can be rapidly obtained through polarization curve testing, meanwhile, the accuracy of the obtained polarization resistance value is guaranteed, and help is provided for aging diagnosis of the high-power SOFC electric pile.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid oxide fuel cells, and in particular to a polarization resistance separation method suitable for large-area anode-supported SOFCs. Background Art

[0002] Solid Oxide Fuel Cell (SOFC) is a highly efficient energy conversion device that has attracted increasing attention due to its fuel flexibility and low emissions. However, the high temperature working environment and complex anode fuel composition will affect the durability of SOFC. Studies have shown that high temperature is one of the main reasons for the agglomeration of metal nickel particles in the anode catalyst. In addition, when the anode fuel is methane, since MSR (Methanesteam reforming reaction) is a strongly endothermic reaction and the electrochemical reaction releases a large amount of heat, this may cause a large temperature gradient inside the SOFC, thereby generating large thermal stress and causing the battery components to fail. Effective diagnosis of how aging factors affect SOFC performance degradation has become the focus of researchers in recent years.

[0003] Electrochemical diagnostic technology has been widely used in SOFC since its development. Constant current or constant voltage test is often used in SOFC calendar life detection, but this test method cannot effectively diagnose the aging mechanism of SOFC. As a traditional electrochemical diagnostic method, polarization curve test is often used to detect the power generation performance of SOFC single cell and stack under different working conditions. It can play a good auxiliary role in helping researchers judge the overall polarization of the battery, but it is difficult to quantify different types of polarization (activation polarization, ohmic polarization, concentration polarization). Electrochemical impedance spectroscopy (EIS) technology can effectively analyze the ion transport and electrochemical process of SOFC under different operating conditions, and obtain various types of impedance in the battery under this condition, but it is difficult to apply EIS test to high-power SOFC stacks due to the output power of the electrochemical workstation.

[0004] Finding a new method to obtain accurate polarization resistance of various types in SOFC by fitting the polarization curve test is a research idea to solve the above problem in recent years. Previously, some scholars introduced Fick's law into the voltage-current relationship, obtained the gas-related polarization resistance by calculating the anode / cathode gas concentration at the three-phase interface, and calculated the activation polarization by the Tafel equation / Butler–Volmer equation to obtain the activation polarization resistance. However, there are three problems in previous studies:

[0005] (1) They are all based on button cells. Since the excess ratio of the gas introduced into the button cell is quite large, they set the gas concentration diffused from the flow channel to the electrode as the inlet concentration of the gas introduced into the battery. In large-area single cells and even battery stacks, economic factors such as fuel / oxygen utilization rate are often considered, so the utilization rate of fuel and oxygen will be controlled within a reasonable range. When a large-area SOFC is running, the reaction gas (H2, O2) in the flow channel will be continuously consumed, and the concentration of the generated gas (H2O) will continue to increase, which will lead to inconsistent distribution of gas concentration in the flow channel and the three-phase reaction interface;

[0006] (2) Under the actual operating conditions of SOFC, at different current densities, the temperature and gas concentration inside the battery will also change due to the different amounts of heat generated and gas consumed, which will lead to differences in the characteristic parameters related to the polarization resistance.

[0007] (3) Gas leakage and electronic conductivity will also have a significant impact on the open circuit voltage and polarization resistance of SOFC. Summary of the invention

[0008] In view of the above-mentioned prior art, the present invention provides a polarization resistance separation method applicable to large-area anode-supported SOFC, and the magnitude of each polarization resistance value can be obtained through polarization curve testing.

[0009] In order to solve the above technical problems, the present invention proposes a polarization resistance separation method suitable for large-area anode-supported SOFC, comprising the following steps:

[0010] Step S1, raising the temperature of the SOFC to the operating state, introducing a certain flow of air and hydrogen into the anode and cathode respectively, and performing a polarization curve test through an electronic load;

[0011] Step S2, establish the relationship between the voltage and current density of the SOFC lumped, the equation is as follows:

[0012]

[0013] In formula (1), V(i) is the voltage of SOFC at different current density i; is the standard Nernst potential, which is related to the battery operating temperature; T is the battery operating temperature; F is the Faraday constant; R is the gas constant; is the partial pressure of O2 at the cathode three-phase interface; is the partial pressure of H2 at the anode three-phase interface; is the partial pressure of H2O at the anode three-phase interface; R i is the sum of the ohmic resistance and the anode charge transfer resistance; is the cathode activation overpotential; It is the electron voltage, which is used to indicate the effect of electron conductivity in the electrolyte membrane on the voltage.

[0014] In calculation and When the membrane electrode is perpendicular to the gas flow channel, the membrane electrode is divided into two regions of equal volume, wherein the region located on the gas inlet side is region 1, and the region located on the gas outlet side is region 2; and The calculation is shown in the following formulas (2)-(4):

[0015]

[0016]

[0017]

[0018] In formula (2) to formula (4), is the partial pressure of O2 leaking from the cathode to the anode, It is the partial pressure consumed by the combustion reaction of H2 introduced into the anode and O2 leaking in at high temperature. is the partial pressure of H2O generated; is the partial pressure of O2 in the gas flow channel at cathode region 1; is the partial pressure of O2 in the gas flow channel at cathode region 2, and the calculation method is shown in formula (5); f and g are parameters related to cathode and anode diffusion and porous electrode properties, respectively; and are the partial pressures of H2 and H2O in the gas flow channel at the anode region 1, respectively; and are the partial pressures of H2 and H2O in the gas flow channel at the anode region 2, respectively. The calculation methods are shown in equations (6) and (7):

[0019]

[0020]

[0021]

[0022] In formula (5) to formula (7), is the volume flow rate of O2 entering the cathode under standard working conditions, Q is the volume flow rate of H2 entering the anode under standard working conditions; Anode and Q Cathode are the gas volume flow rates of the anode and cathode respectively; A is the active area of ​​the battery; n is the number of charges transferred by the electrode reaction; and are the molar masses of O2 and H2 respectively; and are the densities of O2 and H2 introduced into the system under standard working conditions; p is the total gas pressure;

[0023] Couple equations (5)-(7) into equations (2)-(4) respectively, and then couple equations (2)-(4) into equation (1), and the relationship between the voltage and current density of the SOFC lumped is obtained:

[0024]

[0025] Step S3, establish a polarization resistance separation model, use Newton iteration method to fit equation (11) with the polarization curve test results of different current density regions obtained in step S1, and use the model to obtain the following parameters: exchange current density i0, anode limiting current density i al , cathodic limiting current density i cl , the sum of the ohmic resistance and the anode charge transfer resistance R i , leakage volume p L , battery operating temperature T, electronic voltage

[0026] Step S4: setting the concentration difference overpotential η conc Cathodic activation overpotential Take the derivative of i to get the gas concentration resistance R conc and cathode charge transfer resistance As shown in formula (12) and formula (13):

[0027]

[0028]

[0029] Furthermore, the polarization resistance separation method of the present invention, wherein:

[0030] In step 1, the flow rates of air and hydrogen introduced into the anode and cathode respectively are based on the gas flow rates required for the polarization curve test.

[0031] In step S2, the partial pressure is balanced according to the stoichiometric number of the hydrogen combustion reaction. It is expressed as follows:

[0032]

[0033] In step S2, at the limiting current density, or Cathodic limiting current density i cl The relationship between the anode limiting current density i al The relationship with parameter g is shown in formula (9);

[0034]

[0035]

[0036] In step S2, the cathode activation overpotential Calculate according to formula (10):

[0037]

[0038] Where i0 is the exchange current density.

[0039] In step S3, the different current density regions include dividing the current density into a low current density region I and a medium current density region II.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] (1) By adopting the technical solution of the present invention, a relationship between the voltage and current density of the SOFC lumped system is established, and based on this relationship, each polarization resistance can be obtained through polarization curve testing, which provides help for future work on how to improve the power generation performance and durability of large-area SOFCs.

[0042] (2) The technical solution of the present invention can accurately identify the changes in polarization resistance under different current densities, which has a certain guiding significance for studying the change law of polarization resistance of large-area SOFC under operation.

[0043] (3) By adopting the technical solution of the present invention, since the effects of gas leakage and electronic conductivity on voltage are coupled in the model, the installation of battery cells and the performance of the electrolyte membrane can be evaluated. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 The regional division for calculating the gas concentration distribution in the embodiment of the present invention;

[0045] Figure 2 The figure is the fitting of the polarization resistance separation model and the measured polarization curve in the embodiment of the present invention;

[0046] Figure 3 Comparison between the polarization resistance separation model and the EIS test results in the embodiment of the present invention. DETAILED DESCRIPTION

[0047] The present invention proposes a polarization resistance separation method applicable to large-area anode-supported SOFC, which mainly includes the following steps:

[0048] Step S1, the temperature of the activated SOFC is controlled at the operating temperature, a certain volume flow of air and fuel is introduced into the cathode and anode respectively, and the temperature of the introduced gas also needs to be preheated to the operating temperature of the SOFC, and a polarization curve test is carried out.

[0049] Step S2, establishing a relationship between the voltage and current density of the SOFC lumped.

[0050] Step S3, dividing the regions according to the current density, establishing a polarization resistance separation model, that is, fitting the relationship between the voltage and current density of the SOFC lumped with the polarization curve test results, and obtaining various electrochemical parameters according to the results of the model fitting.

[0051] Step S4, the sum of the ohmic resistance and the charge transfer resistance of the anode can be obtained from the electrochemical parameters. i , and based on the addition of R i The electrochemical parameters other than the gas concentration resistance R conc and cathode charge transfer resistance

[0052] The term "large area" in the present invention means that the method is applicable to active areas of (but not limited to) 5×5 cm 2 Up to 11×11cm 2 For SOFCs with a larger range, inspired by the technical solution of the present invention, the method described in the present invention is used for polarization resistance separation of SOFCs with other active areas, which still falls within the scope of protection of the present invention.

[0053] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, but the following embodiments are by no means intended to limit the present invention in any way.

[0054] In this embodiment, the active area is selected to be 10×10 cm 2 The single cell experiment and model fitting are carried out. The polarization resistance separation method suitable for large-area SOFC includes the following steps:

[0055] Step 1, activate the SOFC, then adjust the operating temperature to 750°C, preheat the anode and cathode gases to ensure that the temperature of the anode and cathode gases entering the single cell is 750°C, then introduce 0.5L / min H2+5% Vol H2O into the anode and 1.5L / min air into the cathode. Then use an electronic load to measure the voltage value of the battery under different current operation, and record the voltage value after the voltage stabilizes. In order to verify the accuracy of the model, an EIS test was carried out under the same working conditions. However, in order to avoid the discharge current of the electrochemical workstation exceeding the range, the maximum discharge current of the EIS test was 20A.

[0056] Step 2, establish the relationship between the voltage and current density of the SOFC lumped, the equation is as follows:

[0057]

[0058] In formula (1), V(i) is the voltage of SOFC at different current density i; is the standard Nernst potential, which is related to the battery operating temperature; T is the battery operating temperature; F is the Faraday constant; R is the gas constant; is the partial pressure of O2 at the cathode three-phase interface; is the partial pressure of H2 at the anode three-phase interface; is the partial pressure of H2O at the anode three-phase interface; R i is the sum of the ohmic resistance and the anode charge transfer resistance. As the current density i increases, the heat generated by the battery increases, and the temperature inside the battery also increases. Therefore, R i It decreases with the increase of current density i; is the cathode activation overpotential; It is the electron voltage, which is used to indicate the effect of electron conductivity in the electrolyte membrane on the voltage.

[0059] To couple the influence of the distribution of anode and cathode gases on the gas concentration at the three-phase reaction interface, Figure 1 As shown in the calculation of the partial pressure of each gas at the three-phase reaction interface and When the membrane electrode is divided into two regions of equal volume perpendicular to the gas flow channel, the region located on the gas inlet side is region 1, and the region located on the gas outlet side is region 2. As shown in equations (2) to (4), the average value of the sum of the partial pressures of the gas components at the three-phase interface of regions 1 and 2 is taken as the partial pressure of each gas component at the three-phase reaction interface. and The calculation of is shown in the following formulas (2)-(4):

[0060]

[0061]

[0062]

[0063] In equations (2) to (4), considering the leakage factor, it is assumed that the partial pressure of O2 leaking from the cathode to the anode is The partial pressure consumed by the combustion reaction of H2 introduced into the anode and O2 leaking from the anode at high temperature is The partial pressure of H2O generated is is the partial pressure of O2 at cathode region 1, i.e., the partial pressure of O2 at the cathode inlet; is the partial pressure of O2 at cathode region 2, minus the O2 consumed in region 1, and the calculation method is shown in formula (5); f and g are parameters related to cathode and anode diffusion and porous electrode properties, respectively; and are the partial pressures of H2 and H2O at the anode region 1, i.e., the partial pressures of H2 and H2O at the anode inlet; and are the partial pressures of H2 and H2O at the anode region 2, respectively. The H2 consumed in region 1 is subtracted, and the H2O generated in region 1 is added. The calculation method is shown in equations (6) and (7):

[0064]

[0065] According to the stoichiometric balance of the hydrogen combustion reaction, the partial pressure It is expressed as follows:

[0066]

[0067]

[0068]

[0069] In formula (5) to formula (7), is the volume flow rate of O2 entering the cathode under standard working conditions, Q is the volume flow rate of H2 entering the anode under standard working conditions; Anode and Q Cathode are the gas volume flow rates of the anode and cathode respectively; A is the active area of ​​the battery; n is the number of charges transferred by the electrode reaction; and are the molar masses of O2 and H2 respectively; and are the densities of O2 and H2 introduced into the system under standard working conditions; p is the total gas pressure;

[0070] is the cathode / anode limiting current density i cl / i al and f / g, at the limiting current density ( or ), the O2 / H2 partial pressure in the cathode / anode flow channel is the initial partial pressure of the gas minus half of the gas consumption and gas leakage caused by the emitted current, and the cathode limiting current density i cl The relationship between the anode limiting current density i al The relationship with parameter g is shown in formula (9);

[0071]

[0072]

[0073] Cathodic activation overpotential Calculate according to formula (10):

[0074]

[0075] Where i0 is the exchange current density.

[0076] Substitute equation (8) into equation (2), substitute equation (9) into equation (3) and equation (4), and couple equations (5)-(7) into equations (2)-(4) respectively. Then couple equations (2)-(4) and equation (10) into equation (1), and we get the expressions of SOFC voltage and current density:

[0077]

[0078] Step S3, establish a polarization resistance separation model, and use the Newton iteration method to fit equation (11) with the polarization curve test results obtained in step S1, which are divided into low current density region I and medium current density region II according to the current density. The fitting results are as follows: Figure 2 As shown, various electrochemical parameters can be obtained at the same time, including: exchange current density i0, anode limiting current density i al , cathodic limiting current density i cl , the sum of the ohmic resistance and the anode charge transfer resistance R i , leakage volume p L , battery operating temperature T, electronic voltage

[0079] Step S4: setting the concentration difference overpotential η conc Cathodic activation overpotential Take the derivative of i to get the gas concentration resistance R conc and cathode charge transfer resistance As shown in formula (12) and formula (13):

[0080]

[0081]

[0082] Compare the resistance values ​​obtained by fitting with those obtained by EIS test. Figure 3 The figure shows a comparison between the polarization resistance separation model in the embodiment of the present invention and the EIS test results. It can be observed from the figure that the error is small, which proves that the model of the present invention is highly feasible.

[0083] Although the present invention has been described above in conjunction with the accompanying drawings, the present invention is not limited to the above-mentioned specific embodiments, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can make many improvements and changes without departing from the purpose of the present invention, which are all within the protection of the present invention.

Claims

1. A polarization resistance separation method suitable for large-area anode-supported SOFC, Features: The following steps are involved: Step S1, raising the temperature of the SOFC to the operating state, introducing a certain flow of air and hydrogen into the anode and cathode respectively, and performing a polarization curve test through an electronic load; Step S2, establish the relationship between the voltage and current density of the SOFC lumped, the equation is as follows: In formula (1), V(i) is the voltage of SOFC at different current densities i; V 0 s is the standard Nernst potential, which is related to the battery operating temperature; T is the battery operating temperature; F is the Faraday constant; R is the gas constant; O 2 The partial pressure at the cathode three-phase interface; H 2 The partial pressure at the anode three-phase interface; H 2 The partial pressure of O at the anode three-phase interface; R i is the sum of the ohmic resistance and the anode charge transfer resistance; is the cathode activation overpotential; is the electron voltage, which is used to indicate the effect of the electron conductivity in the electrolyte membrane on the voltage; In calculation and When the membrane electrode is perpendicular to the gas flow channel, the membrane electrode is divided into two regions of equal volume, wherein the region located on the gas inlet side is region 1, and the region located on the gas outlet side is region 2; and The calculation is shown in the following formulas (2)-(4): In formula (2) to formula (4), is O leaking from the cathode to the anode 2 The partial pressure, is the H introduced into the anode 2 At high temperature, the leaked O 2 The partial pressure consumed by the combustion reaction, is the generated H 2 The partial pressure of O; is the O in the gas flow channel at cathode region 1 2 The partial pressure of is the O of the gas flow channel at cathode region 2 2 The partial pressure of is calculated as shown in formula (5); f and g are parameters related to cathode and anode diffusion and porous electrode properties, respectively; and are the H in the gas flow channel at the anode region 1 2 and H 2 The partial pressure of O; and are the H in the gas flow channel at the anode region 2 2 and H 2 The partial pressure of O is calculated as shown in equations (6) and (7): In formula (5) to formula (7), O 2 The volume flow rate into the cathode under standard conditions, H 2 The volume flow rate of the anode under standard conditions; Q Anode and Q Cathode are the gas volume flows entering the anode and cathode respectively; A is the active area of ​​the battery; n is the number of charges transferred by the electrode reaction; and O 2 and H 2 The molar mass of and O 2 and H 2 The density of the gas entering the system under standard working conditions; p is the total gas pressure; Couple equations (5)-(7) into equations (2)-(4) respectively, and then couple equations (2)-(4) into equation (1), and the relationship between the voltage and current density of the SOFC lumped is obtained: Step S3, establish a polarization resistance separation model, use Newton iteration method to fit equation (11) with the polarization curve test results of different current density regions obtained in step S1, and use the model to obtain the following parameters: Exchange current density i 0 , anode limiting current density i al , cathodic limiting current density i cl , the sum of the ohmic resistance and the anode charge transfer resistance R i , leakage volume p L , battery operating temperature T, electronic voltage Step S4, the concentration difference overpotential η conc Cathodic activation overpotential Take the derivative of i to get the gas concentration resistance R conc and cathode charge transfer resistance As shown in formula (13) and formula (14):

2. The polarization resistance separation method according to claim 1, Features: In step 1, the flow rates of air and hydrogen introduced into the anode and cathode respectively are based on the gas flow rates required for the polarization curve test.

3. The polarization resistance separation method according to claim 1, Features: In step S2, the partial pressure is balanced according to the stoichiometric number of the hydrogen combustion reaction. It is expressed as follows: make 4. The polarization resistance separation method according to claim 1, Features: In step S2, at the limiting current density, or Cathodic limiting current density i cl The relationship between the anode limiting current density i al The relationship with parameter g is shown in formula (9); 5. The polarization resistance separation method according to claim 1, Features: In step S2, the cathode activation overpotential According to formula (10), we can get:

6. The polarization resistance separation method according to claim 1, Features: In step S3, the different current density regions include dividing the current density into a low current density region I and a medium current density region II.