Carbon fiber surface treatment method, modified carbon fiber, carbon paper, preparation method of carbon paper and fuel cell
Through non-contact periodic plasma surface treatment and chopping technology, the periodic hydrophobic area of carbon fiber is formed, which solves the problem of non-differential adsorption of adhesives, improves the mechanical properties and breathability of carbon paper, and improves the power generation of fuel cells. performance.
Patent Information
- Application Number
- CN202411123028.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
The existing carbon fiber surface treatment method causes the adhesive to be adsorbed to non-fiber overlapping points in the preparation process of carbon paper, resulting in a decrease in mechanical properties of carbon paper and limited breathability, affecting the reaction mass transfer and drainage channels of fuel cells.
The carbon fiber is chopped by non-contact periodic plasma surface treatment method to form periodic hydrophobic and non-hydrophobic areas, ensuring that each short-cut fiber has at least 2 non-hydrophobic and 2 hydrophobic areas on the surface, and on carbon paper Surfactant and appropriate amount of adhesive are used in preparation to form a porous network structure to improve mechanical properties and breathability.
It effectively improves the mechanical properties and breathability of carbon paper, extends the stability of membrane electrodes and the power generation performance of fuel cells, and avoids the problem of adhesive occupying pore volume, and improves the efficiency of reaction gas conduction and product water discharge.
Smart Images

Figure CN118996833A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and in particular relates to a method for surface treatment of carbon fiber, modified carbon fiber, carbon paper and a preparation method thereof, and a fuel cell. Background Art
[0002] Carbon paper plays the role of supporting the catalyst layer, collecting current, conducting gas and discharging the reaction product water in fuel cells. It is an indispensable key material for fuel cells. Carbon fiber is the main raw material for preparing carbon paper. It is generally made of polyacrylonitrile or viscose fiber as raw materials and is made by high-temperature oxidation and carbonization. Because it has been carbonized at high temperature, its surface inertness is obvious and its functional groups are insufficient. It is generally surface treated before use, and a layer of surfactant is applied on its surface to increase the surface bonding performance of carbon fiber when it is combined with other materials.
[0003] At present, the main methods for carbon fiber surface treatment are: oxidation method, including gas phase oxidation method and liquid phase oxidation method. The gas phase oxidation method uses air or carbon dioxide as an oxidant and reacts at high temperature; the liquid phase oxidation method uses oxidants such as nitric acid or sulfuric acid for treatment, or oxidizes during the electrolysis process to form micropores or etch grooves on the fiber surface, improve surface roughness and introduce polar or reactive functional groups; surface coating method, by depositing a coating on the carbon fiber surface, can reduce surface defects, ease interfacial stress, and enhance the coupling effect between carbon fiber and matrix material; plasma modification, plasma impacts the carbon fiber surface, causing surface oxidation and etching, improving roughness and introducing polar groups, thereby enhancing the bonding strength between carbon fiber and matrix.
[0004] For different application scenarios, the surface treatment methods of carbon fiber are also different. Carbon paper is used as the base material of the gas diffusion layer of hydrogen fuel cells. In the process of preparing carbon fiber paper, it mainly relies on short-cut fibers to overlap each other into a network structure to form a porous material. The connection between the fibers mainly relies on resin adhesives. The mechanical properties of the material mainly rely on its weakest performance, and the performance of carbon paper at the fiber overlap directly determines its mechanical properties. Effective resin / fiber interface connection can not only improve the mechanical properties of carbon paper; reducing ineffective resin aggregation can effectively increase the air permeability and porosity of carbon paper, providing more sufficient mass transfer and drainage channels for fuel cell reactions.
[0005] The existing conventional surface treatment methods are almost all uniform and indiscriminate treatments. Although the effective functional groups on the fiber surface are improved and the cross-sectional bonding strength is increased, during the preparation of carbon paper, the adhesive will be indiscriminately adsorbed on the carbon fiber surface rather than the fiber overlap point. On the one hand, too much adhesive may not improve the mechanical properties of carbon paper; on the other hand, too much adhesive will also occupy a part of the pore volume, thus affecting the comprehensive performance of carbon paper. In short, the "ineffective" adhesive at non-fiber overlap points causes the performance of carbon paper to decline.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The object of the present invention is to provide a method for surface treatment of carbon fiber, modified carbon fiber, carbon paper and preparation method thereof and fuel cell to solve the above problems.
[0008] In order to achieve the above objectives, the present invention particularly adopts the following technical solutions:
[0009] A method for surface treatment of carbon fiber, comprising:
[0010] The carbon fibers are opened, then subjected to plasma surface treatment in a non-contact periodic manner, and then chopped;
[0011] The gas source for the plasma surface treatment is carbon tetrafluoride;
[0012] The chopped carbon fibers satisfy the following condition: (chopped fiber length / fiber running speed) / 4<plasma treatment interval period<(chopped fiber length / fiber running speed) / 2.
[0013] Preferably, the carbon fiber includes one or more of polyacrylonitrile-based carbon fiber, viscose-based carbon fiber, asphalt-based carbon fiber, and lignin-based carbon fiber;
[0014] and / or,
[0015] The diameter of the carbon fiber is 2-8 μm.
[0016] Preferably, the fiber opening process comprises:
[0017] Firstly, air flow is used for blowing, and then the carbon fibers are pressed up and down.
[0018] Preferably, the power of the plasma surface treatment is 50-200w;
[0019] and / or,
[0020] In the non-contact periodic method, a period consists of a processing time and an interval time, and the ratio of the processing time to the interval time is (0.5-2):1.
[0021] Preferably, the aspect ratio of the carbon fiber after chopped carbon fiber is (200-1000):1.
[0022] The present application also provides a modified carbon fiber, which is prepared using the carbon fiber surface treatment method.
[0023] The present application also provides a carbon paper, the raw material of which includes the modified carbon fiber.
[0024] The present application also provides a method for preparing the carbon paper, comprising:
[0025] The modified carbon fiber is wet-dispersed and paper-made to obtain basic carbon paper, and then the basic carbon paper is sprayed with glue, dried, hot-pressed and cured, and carbonized to obtain the carbon paper.
[0026] Preferably, the method for preparing the carbon paper satisfies at least one of the following conditions:
[0027] a. adding a surfactant during the decomposition and papermaking, wherein the surfactant comprises one or more of sodium dodecylbenzene sulfonate, sodium polyacrylate, polyoxyethylene amine, polyethyleneimine, polyoxyethylene alkylphenol, polyvinyl alcohol, polyoxyethylene, polyacrylamide, and carboxymethyl cellulose;
[0028] b. The adhesive applied during the spraying includes one or more of epoxy resin, phenolic resin, polyester resin, bismaleimide, vinyl ester, and polyimide;
[0029] c. The amount of the adhesive applied during the spraying is 25%-75% of the mass of the base carbon paper, calculated by weight after drying;
[0030] d. The carbonization treatment is carried out at a temperature not lower than 1600°C and is carried out under a protective atmosphere.
[0031] The present application also provides a fuel cell, comprising the carbon paper.
[0032] Beneficial effects of the present invention:
[0033] The method for surface treatment of carbon fiber provided in the present application is that when the carbon fiber passes through the plasma surface treatment device continuously, on the one hand, high-energy ions etch the fiber surface to increase the roughness of the fiber surface; on the other hand, the carbon fiber surface is treated with high-energy particles of carbon tetrafluoride, and the fluorocarbon functional groups are significantly increased, which can effectively improve the surface energy of the fiber. After such treatment, the hydrophobicity of the carbon fiber surface is significantly improved. The plasma surface treatment is treated in a non-continuous and periodic manner, that is, the plasma treats the carbon fiber for a period of time, and the plasma treatment is stopped for another period of time; in this way, the surface of the carbon fiber that passes continuously will form periodic hydrophobic areas and non-hydrophobic areas. At the same time, after chopped, the fiber should meet the following conditions: (fiber chopped length / fiber running speed) / 4<plasma treatment interval period<(fiber chopped length / fiber running speed) / 2, to ensure that each section of chopped fiber surface has at least 2 sections of non-hydrophobic areas and 2 sections of hydrophobic areas.
[0034] The method for surface treatment of carbon fiber provided in the present application can, firstly, effectively improve the mechanical properties of the prepared carbon paper without changing the amount of adhesive, further improve the stability and life of the membrane electrode during the membrane electrode equipment process, and effectively increase the power generation performance of the fuel cell. Secondly, without changing the amount of adhesive, the air permeability of the carbon paper can be effectively improved, further during the power generation process, the reaction gas conduction and product water discharge can be effectively improved, and the power generation performance of the fuel cell can also be effectively increased. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0036] Figure 1 Schematic diagram of the structure of carbon paper prepared by plasma surface treatment;
[0037] Figure 2 Schematic diagram of the structure of carbon paper prepared without plasma surface treatment;
[0038] Figure 3 A schematic diagram of the structure of a carbon fiber surface treatment device used in the embodiment;
[0039] Figure 4 It is a comparison diagram of polarization curves of Example 1 and Comparative Example 2.
[0040] Reference numerals:
[0041] 1-non-hydrophobic area of surface-treated carbon fiber; 2-hydrophobic area of surface-treated carbon fiber; 3-unsurface-treated carbon fiber; 4-adhesive;
[0042] 10- Carbon fiber;
[0043] 20-fiber opening device; 21-air blowing plate; 22-fiber opening upper pressure roller; 23-fiber opening lower pressure roller;
[0044] 30-plasma treatment device; 31-plasma emitter; 32-gas source tank; 33-gas circuit;
[0045] 40- shredding device; 41- upper pressing roller for short cutting; 42- lower pressing roller for short cutting; 43- cutting blade. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0047] In order to better explain the present application, the technical solution adopted in the present application is first further described as follows:
[0048] A method for surface treatment of carbon fiber, comprising:
[0049] The carbon fibers are opened, then subjected to plasma surface treatment in a non-contact periodic manner, and then chopped;
[0050] The gas source for the plasma surface treatment is carbon tetrafluoride;
[0051] The chopped carbon fibers satisfy the following condition: (chopped fiber length / fiber running speed) / 4<plasma treatment interval period<(chopped fiber length / fiber running speed) / 2.
[0052] Plasma surface treatment uses the glow discharge principle to form high-energy plasma, and introduces carbon tetrafluoride gas source into the device to form a stable pressure.
[0053] During the dispersion process of carbon paper made from surface-modified carbon fibers, due to the action of surfactants, the non-hydrophobic regions are more likely to overlap with each other to form a porous network structure, in which the non-hydrophobic regions attract each other to form overlapping points. During the spraying and curing process, the adhesive is more likely to accumulate at the resin overlapping points to form bonding points, which can effectively solve the problem of the adhesive being indiscriminately adsorbed on the carbon fiber surface rather than the fiber overlapping points. The schematic diagram of its principle is shown below. Figure 1 As shown in the figure, the structural diagram of carbon paper prepared without plasma surface treatment is as follows Figure 2 shown.
[0054] Short cutting means: the carbon fiber is cut by the cutting device, and then the fiber is transmitted to the cutting head after passing through the upper and lower pressure rollers, and the fiber is cut by the shear force between the cutting head and the lower pressure roller. According to the diameter of the carbon fiber, the gap between the cutting heads is adjusted to control the aspect ratio of the carbon fiber obtained by short cutting.
[0055] In an optional embodiment, the carbon fiber includes one or more of polyacrylonitrile-based carbon fiber, viscose-based carbon fiber, asphalt-based carbon fiber, and lignin-based carbon fiber;
[0056] and / or,
[0057] The diameter of the carbon fiber is 2-8 μm.
[0058] Optionally, the diameter of the carbon fiber may be 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm or any value between 2 and 8 μm.
[0059] In an optional embodiment, the fiber opening process includes:
[0060] Firstly, air flow is used for blowing, and then the carbon fibers are pressed up and down.
[0061] First, air blowing is used to increase the width and reaction contact area, and then the upper and lower pressure rollers are used to press the opened carbon fibers to form a continuous and stable running speed and maintain tension.
[0062] In an optional embodiment, the power of the plasma surface treatment is 50-200w;
[0063] and / or,
[0064] In the non-contact periodic method, a period consists of a processing time and an interval time, and the ratio of the processing time to the interval time is (0.5-2):1.
[0065] Optionally, the power of the plasma surface treatment can be 50w, 100w, 150w, 200w or any value between 50-200w; the ratio of the treatment time to the interval time can be 0.5:1, 1:1, 1.5:1, 2:1 or any value between (0.5-2):1.
[0066] In an optional embodiment, the aspect ratio of the carbon fiber after chopped carbon fiber is (200-1000):1.
[0067] Optionally, the aspect ratio of the carbon fiber after chopped carbon fiber can be 200:1, 300:1, 400:1, 500:1, 600:1, 700:1, 800:1, 900:1, 1000:1 or any value between (200-1000):1.
[0068] The present application also provides a modified carbon fiber, which is prepared using the carbon fiber surface treatment method.
[0069] The present application also provides a carbon paper, the raw material of which includes the modified carbon fiber.
[0070] The present application also provides a method for preparing the carbon paper, comprising:
[0071] The modified carbon fiber is wet-dispersed and paper-made to obtain basic carbon paper, and then the basic carbon paper is sprayed with glue, dried, hot-pressed and cured, and carbonized to obtain the carbon paper.
[0072] In an optional embodiment, the method for preparing the carbon paper satisfies at least one of the following conditions:
[0073] a. adding a surfactant during the decomposition and papermaking, wherein the surfactant comprises one or more of sodium dodecylbenzene sulfonate, sodium polyacrylate, polyoxyethylene amine, polyethyleneimine, polyoxyethylene alkylphenol, polyvinyl alcohol, polyoxyethylene, polyacrylamide, and carboxymethyl cellulose;
[0074] According to the double-layer adsorption theory, surfactants are easily adsorbed on the surface of the non-hydrophobic region of carbon fiber, so that the non-hydrophobic regions of different fibers are more likely to overlap with each other to form a porous network structure.
[0075] b. The adhesive applied during the spraying includes one or more of epoxy resin, phenolic resin, polyester resin, bismaleimide, vinyl ester, and polyimide;
[0076] After applying the adhesive, the fiber connection points in the carbon paper should be well connected without peeling, cracking, falling off, etc.
[0077] c. The amount of the adhesive applied during the spraying is 25%-75% of the mass of the base carbon paper, calculated by weight after drying;
[0078] Optionally, the amount of the adhesive applied during the spraying may be 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or any value between 25% and 75% of the mass of the base carbon paper;
[0079] d. The carbonization treatment is carried out at a temperature not lower than 1600°C and is carried out under a protective atmosphere.
[0080] The curing of carbon paper should meet the curing conditions of the adhesive; the carbonization temperature of carbon paper should not be lower than 1600°C, and it should be protected by, for example, a nitrogen atmosphere to prevent oxidation at high temperature from damaging the carbon paper.
[0081] The present application also provides a fuel cell, comprising the carbon paper.
[0082] In order to better describe the technical solution of the present application, the equipment used in the embodiment is described below, as follows:
[0083] like Figure 3As shown, the surface treatment device for treating carbon fiber 10 includes a fiber opening device 20, a plasma treatment device 30, and a slicing device 40; wherein the fiber opening device 20 includes an air flow blowing plate 21, an upper fiber opening roller 22, and a lower fiber opening roller 23; the plasma treatment device 30 includes a plasma emitter 31, an air source storage tank 32, and an air path 33; the slicing device 40 includes a short-cut upper roller 41, a short-cut lower roller 42, and a cutting blade 43. In the figure, the product is a modified carbon fiber 50 after short-cutting.
[0084] Example 1
[0085] This embodiment provides a method for surface treatment of carbon fiber, combined with the above device, the specific steps are as follows:
[0086] First, the carbon fiber 10 is passed through the fiber opening device 20 along the conveyor belt to make the fiber bundles dispersed well; then the surface treatment is carried out by the plasma treatment device 30, and this surface treatment is a non-contact periodic intermittent treatment; then the continuous carbon fiber is chopped by the slitting device 40 for standby use;
[0087] The carbon fiber can be continuously transported through the front and rear two-stage pressing rollers; the carbon fiber 10 to be processed first passes through the fiber opening device 20 to make the fiber bundles well dispersed; then the carbon fiber passes through the plasma treatment device 30, using carbon tetrafluoride as the gas source and controlling the plasma treatment power to 120W and the plasma treatment interval period to 0.12S, wherein the treatment time is 0.06S and the interval time is 0.06S; then the continuous carbon fiber is chopped using the filament cutting device 40, and the aspect ratio of the chopped fiber is controlled to be 750:1 according to the fiber diameter, and the chopped fiber is prepared for standby use.
[0088] The chopped fibers were decomposed, dehydrated and paper-made in water containing 0.5% sodium polyacrylate; the glue was sprayed with a solution containing 3% phenolic resin, and after drying, the glue application amount was controlled to be 40% of the weight of the carbon paper; the carbon paper was then hot-pressed at 170°C for 20 minutes to complete curing; finally, the carbon paper was placed in a high-temperature carbonization furnace and carbonized to 1600°C under nitrogen protection to complete the preparation of the carbon paper.
[0089] Embodiment 2-6
[0090] During the preparation process, the ion treatment power, ion treatment interval period, fiber aspect ratio after chopped fiber, and sizing amount parameters were changed. Other conditions were the same as those in Example 1 for carbon fiber surface treatment and carbon paper preparation. The specific preparation conditions are shown in Table 1 below.
[0091] Comparative Example 1-2
[0092] During the preparation process, the carbon fiber was not subjected to plasma surface treatment. Other conditions were the same as those in Example 1 for carbon fiber surface treatment and carbon paper preparation. The specific preparation conditions are shown in Table 1 below.
[0093] Table 1 Process parameters
[0094]
[0095] The carbon papers prepared in all the examples and comparative examples were tested for performance, including the tensile strength, compression rate (1 MPa), and air permeability of the carbon papers. The results are shown in Table 2 below:
[0096] Table 2 Test results
[0097]
[0098]
[0099] Compared with Example 1, since the carbon fiber in Example 1 has not been subjected to plasma surface treatment, the hydrophobicity of the fiber surface is uniform. During the process of spraying and curing the carbon paper, the adhesive will randomly and indiscriminately combine with any position of the carbon fiber, resulting in a large distribution of adhesive at non-fiber overlap points, which not only fails to enhance the mechanical properties of the carbon paper, but on the contrary will occupy part of the pore space and reduce the air permeability of the carbon paper. In Example 1, due to the intermittent plasma surface treatment, discontinuous hydrophobic areas and non-hydrophobic areas are formed on the surface of the chopped fibers. Firstly, during the papermaking process, due to the presence of surfactants, these non-hydrophobic areas are more likely to attract each other to form fiber overlap points; further, during the adhesive spraying and curing process, due to the high roughness and large surface energy of the hydrophobic areas on the fiber surface, the adhesive gathers to the non-hydrophobic areas (fiber overlap points) and forms stable spheroids as much as possible. In this way, the effective adhesive content at the fiber overlap points is greatly increased compared with that in Comparative Example 1, and the mechanical properties are also significantly improved; on the other hand, since the adhesive only exists in the fiber overlap points in the form of the smallest volume, the pore structure between the fibers will be greatly retained, and it can be seen that the air permeability of Example 1 is significantly increased compared with Comparative Example 1.
[0100] Compared with Example 1 and Comparative Example 2, although Comparative Example 2 improves the mechanical properties to a certain extent by increasing the amount of adhesive applied, and the tensile strength and compression rate are basically consistent with those of Example 1, the amount of adhesive applied is too large and not well distributed, and the "ineffective" adhesive occupies more pore structures, causing the air permeability to further decrease.
[0101] After the carbon paper prepared in Example 1 and Comparative Example 2 is further impregnated with 12% polytetrafluoroethylene emulsion, a 30 μm microporous layer (containing conductive carbon black and polytetrafluoroethylene hydrophobic agent) is coated on one side and sintered at 350°C for 30 minutes to complete the preparation of the gas diffusion layer. The hydrogen fuel cell membrane electrode is assembled in the manner of anode gas diffusion layer, anode catalyst, proton exchange membrane, cathode catalyst, and cathode gas diffusion layer. After being fixed in a fixture, it is connected to the test system for single cell testing. The test conditions are as follows: battery temperature 75°C, cathode and anode relative humidity 100% RH, cathode is air (stoichiometric ratio 2.5), anode is hydrogen (stoichiometric ratio 1.2), cathode and anode back pressure 50 kPa, and then the polarization curve test is completed. The results are as follows Figure 4 shown.
[0102] Depend on Figure 4 It can be seen that when the voltage of Example 1 and Comparative Example 2 is above 0.5V, the battery performance is basically the same. However, at a low voltage of less than 0.5V, as the current density increases, the water discharged from the membrane electrode gradually increases, and it is bound to occupy a certain pore channel. Since the binder in Comparative Example 2 is randomly distributed and occupies a certain pore space, the pores left for the reaction gas to conduct are relatively reduced due to the influence of drainage at low voltage, and the power generation efficiency is significantly reduced. Its maximum power density is 0.89W / cm 2 However, in Example 1, there is no such obvious effect at low voltage. Due to the large air permeability of the gas diffusion layer, the adhesive is distributed in the form of minimum volume at the fiber overlap point, more pore structures are retained, and the slope of the polarization curve remains constant without obvious decrease. Its maximum power density can reach 1.06W / cm 2 .
[0103] Please note that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above embodiments only express several implementation methods of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several variations and improvements can be made, which all belong to the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the attached claims.
Claims
1. A method for surface treatment of carbon fiber, characterized in that: include: The carbon fibers are opened, then subjected to plasma surface treatment in a non-contact periodic manner, and then chopped; The gas source for the plasma surface treatment is carbon tetrafluoride; The chopped carbon fibers satisfy the following condition: (chopped fiber length / fiber running speed) / 4<plasma treatment interval period<(chopped fiber length / fiber running speed) / 2.
2. The method for surface treatment of carbon fiber according to claim 1, characterized in that: The carbon fiber includes one or more of polyacrylonitrile-based carbon fiber, viscose-based carbon fiber, asphalt-based carbon fiber, and lignin-based carbon fiber; And / or, the diameter of the carbon fiber is 2-8 μm.
3. The method for surface treatment of carbon fiber according to claim 1, characterized in that: The fiber opening process includes: firstly using air flow to blow, and then pressing the carbon fibers up and down.
4. The method for surface treatment of carbon fiber according to claim 1, characterized in that: The power of the plasma surface treatment is 50-200w; and / or, In the non-contact periodic method, a period consists of a processing time and an interval time, and the ratio of the processing time to the interval time is (0.5-2):
1.
5. The method for surface treatment of carbon fiber according to any one of claims 1 to 4, characterized in that: The aspect ratio of the chopped carbon fiber is (200-1000):
1.
6. A modified carbon fiber, characterized in that: The carbon fiber is prepared by the method for surface treatment of carbon fiber according to any one of claims 1 to 5.
7. A carbon paper, characterized in that: The raw material includes the modified carbon fiber described in claim 6.
8. A method for preparing carbon paper according to claim 7, characterized in that: include: The modified carbon fiber is wet-processed for decomposition and papermaking to obtain basic carbon paper, and then the basic carbon paper is subjected to glue spraying, drying, hot pressing curing treatment and carbonization treatment to obtain the carbon paper.
9. The method for preparing carbon paper according to claim 8, characterized in that: At least one of the following conditions is met: a. adding a surfactant during the decomposition and papermaking, wherein the surfactant comprises one or more of sodium dodecylbenzene sulfonate, sodium polyacrylate, polyoxyethylene amine, polyethyleneimine, polyoxyethylene alkylphenol, polyvinyl alcohol, polyoxyethylene, polyacrylamide, and carboxymethyl cellulose; b. The adhesive applied during the spraying includes one or more of epoxy resin, phenolic resin, polyester resin, bismaleimide, vinyl ester, and polyimide; c. The amount of the adhesive applied during the spraying is 25%-75% of the mass of the base carbon paper, calculated by weight after drying; d. The carbonization treatment is carried out at a temperature not lower than 1600°C and is carried out under a protective atmosphere.
10. A fuel cell, characterized in that: Comprising the carbon paper as claimed in claim 7.