Preparation method and application of electrolyte containing LiFSI
By using lithium difluorosulfonimide (LiFSI) as a new lithium salt in lithium-ion batteries, the preparation of LiFSI-containing electrolyte solution was solved, and the low-temperature and rate performance of lithium-ion batteries was significantly improved. However, High temperature performance has certain negative effects.
Patent Information
- Application Number
- CN202411077144.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Lithium-ion batteries have poor performance at low temperatures and rate magnifications, and the price of lithium hexafluorophosphate is rising, so we are looking for a new lithium salt alternative to improve electrochemical performance.
Lithium difluorosulfonimide (LiFSI) is used as a new lithium salt, and the LiFSI-containing electrolyte is prepared by stirring with lithium hexafluorophosphate and mixed solvent in a glove box filled with argon, and the lithium hexafluorosulfonimide and lithium hexafluorophosphate are controlled. The mass fraction is between 2 and 10.5%, which is used to improve the low temperature and rate performance of lithium-ion batteries.
It significantly reduces the viscosity of the electrolyte and improves the conductivity, improves the low-temperature discharge performance and rate performance, but has little impact on the internal resistance and cycling performance of the room temperature. In addition, the aluminum foil will be corroded when replaced by all LiFSI, deteriorates the high-temperature storage and cycling performance.
Smart Images

Figure CN118983536A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery electrolytes, and in particular to a preparation method and application of an electrolyte containing LiFSI. Background Art
[0002] With the rapid development of science and technology, human demand for energy has increased dramatically. With the increasing depletion of fossil energy such as coal and oil, natural energy such as wind energy and solar energy cannot be used stably. Efficient, clean, safe and reusable new energy has become the focus of attention of all mankind. Lithium-ion batteries have the advantages of high energy density, no memory effect, long service life, clean and pollution-free, and are widely used in various fields, including mobile phones, laptops, new energy vehicles and other fields. As a key part of lithium-ion batteries, electrolyte has an important impact on the performance of lithium-ion batteries. Lithium hexafluorophosphate, a lithium salt, has the advantages of high ion conductivity and good solubility. It is still a widely used lithium salt in commercialization, but lithium hexafluorophosphate has poor thermal stability and is very sensitive to water and easily decomposes to produce HF. In addition, the price of lithium hexafluorophosphate has continued to rise recently, so a new type of lithium salt is sought to replace lithium hexafluorophosphate. Lithium bis(fluorosulfonyl)imide LiFSI has many advantages such as high safety, high stability, high conductivity and wide electrochemical window, which can improve the low temperature performance and rate performance of lithium-ion batteries. In addition, LiFSI is currently inexpensive, so using the new lithium salt LiFSI to partially replace lithium hexafluorophosphate is an effective way to improve the electrochemical performance of lithium-ion batteries. Summary of the invention
[0003] The invention provides a method for preparing an electrolyte containing LiFSI, which solves the problems of poor low temperature performance, rate performance and the like of lithium ion batteries.
[0004] The technical solution provided by the present invention is: a method for preparing an electrolyte containing LiFSI: in a glove box filled with argon, adding a mixed solvent, lithium hexafluorophosphate, and lithium bis(fluorosulfonyl)imide into a container, stirring and mixing, to obtain an electrolyte containing LiFSI.
[0005] The mass fraction of lithium bis(fluorosulfonyl)imide in the electrolyte is 2-10.5%, and the mass fraction of lithium hexafluorophosphate is 2-10.5%.
[0006] Preferably, the total mass fraction of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide in the electrolyte is 14%.
[0007] Preferably, the mixed solvent consists of ethylene carbonate, propylene carbonate, diethyl carbonate and dimethyl carbonate.
[0008] Preferably, the mass ratio of ethylene carbonate, propylene carbonate, diethyl carbonate and dimethyl carbonate in the mixed solvent is 30:5:40:25.
[0009] Preferably, the lithium-ion battery containing the electrolyte of LiFSI is composed of a positive electrode, a negative electrode, an electrolyte containing LiFSI, and a separator.
[0010] Preferably, the positive electrode is lithium iron phosphate, the negative electrode is natural graphite, and the separator is a PE separator.
[0011] Preferably, a method for preparing a lithium-ion battery having an electrolyte containing LiFSI is as follows: the positive electrode lithium iron phosphate and the negative electrode natural graphite are die-cut respectively to make positive and negative electrode sheets, and then the positive and negative electrode sheets are laminated with a PE diaphragm into a soft-pack battery cell, and then the cells are welded, glued, assembled, injected with electrolyte, formed, molded, and capacity divided to obtain a lithium-ion battery.
[0012] The technical effect of the present invention is that the mixed lithium salt adding LiFSI can reduce the viscosity of the electrolyte and improve the conductivity. When the LiFSI content reaches 10.5%, that is, the lithium salt content is more than 84%, the low-temperature internal resistance can be significantly reduced, and the low-temperature discharge performance and normal temperature rate performance can be effectively improved, but it has little effect on the normal temperature internal resistance and normal temperature cycle. In addition, when all LiFSI is replaced, it will corrode the aluminum foil and deteriorate the high-temperature storage and high-temperature cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a test of the viscosity of the electrolyte at different temperatures.
[0014] Figure 2 It is a test of the conductivity of the electrolyte at different temperatures.
[0015] Figure 3 It is a DCIR test of lithium-ion battery discharge at different temperatures.
[0016] Figure 4 It is a lithium-ion battery discharge test at different rates at 25°C.
[0017] Figure 5 It is a lithium-ion battery storage test at 60°C.
[0018] Figure 6 It is a lithium-ion battery cycle performance test.
[0019] Figure 7 This is the SEM test of aluminum foil at the end of the cycle. DETAILED DESCRIPTION
[0020] The technical solution of the present invention will be clearly and completely described below through the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0021] Example 1
[0022] This embodiment is referred to as Scheme B.
[0023] In a glove box filled with argon, ethylene carbonate, propylene carbonate, diethyl carbonate, and dimethyl carbonate in a mass ratio of 30:5:40:25 were added to the container as a mixed solvent, and then lithium hexafluorophosphate and lithium bisfluorosulfonyl imide were added and stirred to obtain an electrolyte containing LiFSI. The mass fraction of lithium bisfluorosulfonyl imide in the electrolyte was controlled to be 2%, and the mass fraction of lithium hexafluorophosphate was 10.5%.
[0024] The positive electrode lithium iron phosphate and the negative electrode natural graphite are die-cut separately to make positive and negative electrode sheets, and then the positive and negative electrode sheets are stacked with PE separators to form soft-pack battery cells, which are then welded, glued, assembled, injected with electrolyte, formed, molded, and divided into volumes to obtain lithium-ion batteries.
[0025] Example 2
[0026] This embodiment is referred to as Scheme C.
[0027] In a glove box filled with argon, ethylene carbonate, propylene carbonate, diethyl carbonate, and dimethyl carbonate in a mass ratio of 30:5:40:25 were added to the container as a mixed solvent, and then lithium hexafluorophosphate and lithium bisfluorosulfonyl imide were added and stirred to obtain an electrolyte containing LiFSI. The mass fraction of lithium bisfluorosulfonyl imide in the electrolyte was controlled to be 3.5%, and the mass fraction of lithium hexafluorophosphate was 9%.
[0028] The positive electrode lithium iron phosphate and the negative electrode natural graphite are die-cut separately to make positive and negative electrode sheets, and then the positive and negative electrode sheets are stacked with PE separators to form soft-pack battery cells, which are then welded, glued, assembled, injected with electrolyte, formed, molded, and divided into volumes to obtain lithium-ion batteries.
[0029] Example 3
[0030] This embodiment is referred to as Scheme D.
[0031] In a glove box filled with argon, ethylene carbonate, propylene carbonate, diethyl carbonate, and dimethyl carbonate in a mass ratio of 30:5:40:25 were added to the container as a mixed solvent, and then lithium hexafluorophosphate and lithium bisfluorosulfonyl imide were added and stirred to obtain an electrolyte containing LiFSI. The mass fraction of lithium bisfluorosulfonyl imide in the electrolyte was controlled to be 6%, and the mass fraction of lithium hexafluorophosphate was 6.5%.
[0032] The positive electrode lithium iron phosphate and the negative electrode natural graphite are die-cut separately to make positive and negative electrode sheets, and then the positive and negative electrode sheets are stacked with PE separators to form soft-pack battery cells, which are then welded, glued, assembled, injected with electrolyte, formed, molded, and divided into volumes to obtain lithium-ion batteries.
[0033] Example 4
[0034] This embodiment is referred to as Scheme E.
[0035] In a glove box filled with argon, ethylene carbonate, propylene carbonate, diethyl carbonate, and dimethyl carbonate in a mass ratio of 30:5:40:25 were added to the container as a mixed solvent, and then lithium hexafluorophosphate and lithium bisfluorosulfonyl imide were added and stirred to obtain an electrolyte containing LiFSI. The mass fraction of lithium bisfluorosulfonyl imide in the electrolyte was controlled to be 10.5%, and the mass fraction of lithium hexafluorophosphate was 2%.
[0036] The positive electrode lithium iron phosphate and the negative electrode natural graphite are die-cut separately to make positive and negative electrode sheets, and then the positive and negative electrode sheets are stacked with PE separators to form soft-pack battery cells, which are then welded, glued, assembled, injected with electrolyte, formed, molded, and divided into volumes to obtain lithium-ion batteries.
[0037] Comparative Example 1
[0038] This embodiment is referred to as Scheme A.
[0039] In a glove box filled with argon, ethylene carbonate, propylene carbonate, diethyl carbonate, and dimethyl carbonate in a mass ratio of 30:5:40:25 were added to a container as a mixed solvent, and then lithium hexafluorophosphate was added and stirred to obtain an electrolyte. The mass fraction of lithium hexafluorophosphate was controlled to be 12%.
[0040] The positive electrode lithium iron phosphate and the negative electrode natural graphite are die-cut separately to make positive and negative electrode sheets, and then the positive and negative electrode sheets are stacked with PE separators to form soft-pack battery cells, which are then welded, glued, assembled, injected with electrolyte, formed, molded, and divided into volumes to obtain lithium-ion batteries.
[0041] Comparative Example 2
[0042] This embodiment is referred to as Scheme F.
[0043] In a glove box filled with argon, ethylene carbonate, propylene carbonate, diethyl carbonate, and dimethyl carbonate in a mass ratio of 30:5:40:25 were added to the container as a mixed solvent, and then lithium bis(fluorosulfonyl)imide was added and stirred to obtain an electrolyte containing LiFSI. The mass fraction of lithium bis(fluorosulfonyl)imide in the electrolyte was controlled to be 12%.
[0044] The positive electrode lithium iron phosphate and the negative electrode natural graphite are die-cut separately to make positive and negative electrode sheets, and then the positive and negative electrode sheets are stacked with PE separators to form soft-pack battery cells, which are then welded, glued, assembled, injected with electrolyte, formed, molded, and divided into volumes to obtain lithium-ion batteries.
[0045] Electrolyte viscosity and conductivity test: Use Ostwald viscometer ( The viscometer constant is 0.02726 mm 2 / s 2 ) Test the viscosity of the electrolyte at different temperatures, and use a conductivity meter (Mettler-Torido conductivity meter FE-30) to detect the conductivity of the electrolyte at different temperatures. The test temperature is -30℃~45℃.
[0046] A high-precision battery system was used to test the DC internal resistance of the battery. The test conditions were as follows: charge and discharge at 0.5C for 5 weeks at 25±2℃, with a voltage range of 2.5 to 3.65V, and then discharged at 0.33C to (2.0V) / (2.5V) at (-10℃±2℃, 0℃±2℃) / (10℃±2℃, 45℃±2℃), and the capacity Q was recorded; then placed at 25±2℃ and charged and discharged at 0.5C for 3 weeks for capacity recovery; the battery was charged at 0.5C to 100% SOC at 25±2℃, and the battery was placed to ambient temperature at -10℃±2℃ / 0℃±2℃ / 10℃±2℃ / 45℃±2℃, and the battery was discharged at 0.33C, and the battery capacity was adjusted to the measured SOC according to the calibrated capacity Q; placed for 1h, the battery was charged at 1.0C.
[0047] Calculation of DC internal resistance (DCIR): After adjusting the SOC, leave it for 1 hour, and the terminal voltage is recorded as V0. Discharge at a constant current of 1.0C for 60 seconds, and the terminal voltage is V1. Discharge: DCIR = (V0-V1) / I. Calculate the DCIR of 90% SOC, 70% SOC, 50% SOC, and 30% SOC respectively.
[0048] Rate discharge test: A high-precision battery system is used to test the room temperature rate performance of the battery. The test conditions are: the battery is charged to 3.65V at 0.5C constant current and constant voltage at 25±2℃, then discharged to 2.5V at 0.1C constant current, and the discharge energy and median voltage are recorded. Then, the battery is charged to 3.65V at 0.5C constant current and constant voltage, then discharged to 2.5V at 0.2C constant current, and the discharge energy and median voltage are recorded. This is repeated, and the discharge energy and median voltage of 0.5C, 1C, 2C, and 3C are recorded respectively. The ratio of the discharge energy of 0.1C, 0.2C, 0.5C, 1C, 2C, and 3C to the discharge energy of 0.1C is the rate performance of the current.
[0049] Discharge test at different temperatures: A high-precision battery system and a high and low temperature test alternating box (Dongguan Bell Test Equipment Co., Ltd.) were used to test the low-temperature discharge performance of the battery. The test conditions were as follows: the battery was charged to 3.65V at 0.1C constant current and constant voltage at 25±2℃, then discharged to 2.5V at 0.1C constant current, and the normal temperature discharge capacity was recorded. The test battery was then fully charged, placed at 0℃ for 24h, and then discharged to 2.0V at 0.1C, and the discharge capacity and median voltage were recorded. The capacity ratio of the two is the discharge performance at 0℃. Similarly, the discharge performance at -20℃ and -30℃ was tested respectively.
[0050] 60℃ storage test: A high-precision battery system and a high and low temperature test alternating box (Dongguan Bell Testing Equipment Co., Ltd.) were used to test the high-temperature storage performance of the battery. The test conditions were as follows: the battery was charged to 3.65V at 0.5C constant current and constant voltage at 25±2℃, then discharged to 2.5V at 0.5C constant current, and the initial discharge capacity was recorded. The test battery was then fully charged, placed at 60℃ for 30d, and then discharged to 2.5V at 0.5C, and the remaining discharge capacity was recorded. The ratio of the remaining discharge capacity to the initial capacity was calculated, which was the capacity retention rate. The battery was then charged to 3.65V at 0.5C constant current and constant voltage at 25±2℃, and then discharged to 2.5V at 0.5C constant current, and the recovery discharge capacity was recorded. The ratio of the recovery discharge capacity to the initial capacity was calculated, which was the capacity recovery rate.
[0051] Cycle performance test: A high-precision battery system is used to test the cycle performance of the battery. The test conditions are: charge to 3.65V at room temperature with 1C constant current and constant voltage, then discharge to 2.5V with 1C constant current, perform cycle test, and calculate the capacity retention rate. The cycle performance of 45℃ 1C charge and discharge is also tested.
[0052] SEM test of aluminum foil at the end of the cycle: A Czech TESCAN Brno.sro scanning electron microscope was used to observe the aluminum foil at the end of the cycle. The battery that had been cycled for 1500 cycles at 45°C was disassembled and the aluminum foil was obtained and observed using a scanning electron microscope.
[0053] Electrolyte viscosity analysis: The electrolyte viscosity test results at different temperatures are as follows: Figure 1 As shown in the figure, at the same temperature, the viscosity of the F scheme (all LiFSI) is smaller than that of the A scheme (all LiPF6), and the viscosity gradually decreases as the proportion of LiFSI increases; the viscosity at low temperature of -30°C decreases significantly as the proportion of LiFSI increases, and the F (all LiFSI) is the lowest, almost 1 / 3 of the full LiPF6 scheme; the F scheme (all LiFSI) decreases very little as the temperature increases from -30°C to 45°C. This shows that the addition of LiFSI to the electrolyte can effectively reduce the viscosity, because the bis(fluorosulfonyl)imide anion has a weaker coordination with the lithium ion, which is beneficial to the ionization of the lithium ion, resulting in a decrease in the viscosity of the electrolyte.
[0054] Electrolyte conductivity analysis: Conductivity is an important characteristic of electrolyte, which affects many electrochemical properties of lithium-ion batteries. Figure 2 The results of the conductivity test of the electrolyte at different temperatures are shown in the figure. As can be seen from the figure, at the same temperature, the conductivity of the F scheme (all LiFSI) is higher than that of the A scheme (all LiPF6). As the proportion of LiFSI increases, the conductivity gradually increases; as the temperature decreases from 45°C to -30°C, the lower the temperature, the higher the proportion of LiFSI, and the conductivity increases significantly. This shows that adding LiFSI to the electrolyte can effectively improve the conductivity. This is because the bis(fluorosulfonyl)imide anion added to LiFSI has a larger anion radius, resulting in a large dissociation constant and a larger number of lithium ions that are deintercalated, which can effectively improve the conductivity of the electrolyte.
[0055] Lithium-ion battery discharge DCIR test at different temperatures: Figure 3 (a) is the DCIR test result of -10℃ discharge. Figure 3 (b) is the DCIR test result of 0℃ discharge. Figure 3 (c) is the DCIR test result of 10℃ discharge. Figure 3 (d) is the DCIR test result of discharge at 25℃.
[0056] Depend on Figure 3 (a) It can be seen that at -10℃, the discharge DCIR of different charge states of schemes A, B, and C differ by 1 to 5 mΩ. As the proportion of LiFSI increases, the discharge DCIR of different charge states of schemes D, E, and F decreases significantly. The discharge DCIR of different charge states of scheme F (full LiFSI) is smaller than that of scheme A (full LiPF6), and the difference between the two is 25 to 28 mΩ.
[0057] Depend on Figure 3 (b) It can be seen that the discharge DCIR of different charge states of schemes A, B, and C differ by 0 to 3 mΩ. As the proportion of LiFSI increases, the discharge DCIR of different charge states of schemes D, E, and F decreases significantly. The discharge DCIR of different charge states of scheme F (full LiFSI) is smaller than that of scheme A (full LiPF6), and the difference between the two is 28 to 30 mΩ.
[0058] Depend on Figure 3 (c) It can be seen that the discharge DCIR of different charge states of schemes A, B, and C differ by 0 to 2 mΩ. As the proportion of LiFSI increases, the discharge DCIR of different charge states of schemes D, E, and F decreases. The discharge DCIR of different charge states of schemes D, E, and F differ by 1 to 3 mΩ. The discharge DCIR of different charge states of scheme F (full LiFSI) is smaller than that of scheme A (full LiPF6), and the difference between the two is 12 to 14 mΩ.
[0059] Depend on Figure 3 (d) It can be seen that the discharge DCIR of different charge states of schemes A, B, C, E, and F differ by 0 to 3 mΩ, and the discharge DCIR of different charge states of each scheme does not change significantly, which is consistent with the conductivity and viscosity test results of the electrolyte at room temperature in the previous article.
[0060] The above shows that when the LiFSI content reaches more than 6.0%, that is, more than 48% of the lithium salt content, the low-temperature discharge DCIR can be significantly reduced, and the lower the temperature, the more obvious the DCIR reduction, but it has little effect on the normal temperature discharge DCIR, which is consistent with the conductivity and viscosity test results of the electrolyte at room temperature in the previous article.
[0061] 25℃ different rate discharge test: Figure 4 (a) is the median discharge voltage at different rates at 25℃. Figure 4 (b) is the discharge energy efficiency at different rates at 25°C.
[0062] Depend on Figure 4 (a) and (b) show that the addition of LiFSI has little effect on the median voltage of different discharge rates at room temperature, but the energy efficiency is quite different when discharging at 1C, 2C, and 3C. When discharging at 1-3C, the discharge energy efficiency of the E scheme (10.5% LiFSI) is the highest, and the energy efficiency of the A (full LiPF6) scheme is the lowest, which shows that the addition of LiFSI has a certain improvement on the rate discharge performance. The rate performance of the battery is related to the conductivity and viscosity of the electrolyte, which is the main reason why the rate performance of LiPF6 / LiFSI is better than that of pure LiPF6.
[0063] Discharge test at different temperatures: Table 1 shows the test results of discharge at different temperatures. It can be seen from Table 1 that, 0℃-0.1C discharge: Scheme B has the lowest capacity retention rate and median voltage, and Schemes D to F (with a higher proportion of LiFSI) have a capacity retention rate increased by 0.21% to 1.23%, and a median voltage increased by 5 to 9 mV; -20℃-0.1C discharge: Scheme B has the lowest capacity retention rate and median voltage, and Schemes D to F (with a higher proportion of LiFSI) have a capacity retention rate increased by 1.64% to 3.71%, and a median voltage increased by 31 to 61 mV; -30℃-0.1C discharge: Scheme B has the lowest capacity retention rate and median voltage, and Schemes D to F (with a higher proportion of LiFSI) have a capacity retention rate increased by 1.98% to 4.85%, and a median voltage increased by 47 to 87 mV; In addition, the lower the temperature, the more obvious the improvement in low-temperature performance is when LiFSI is added.
[0064] The low temperature performance of the battery is closely related to the low temperature conductivity and low temperature viscosity of the electrolyte. Generally speaking, the lower the viscosity of the electrolyte at low temperature, the higher the conductivity, and the better the low temperature discharge performance. This is roughly consistent with the above Figure 1 , Figure 2 , Figure 3 (a) Figure 3 The test results of (b) are consistent. This fully demonstrates that the addition of LiFSI mixed lithium salt can improve the low temperature performance of lithium-ion batteries.
[0065]
[0066] 60℃ storage test: Figure 5 (a) Capacity retention and recovery rate of storage at 60℃ for 30 days, Figure 5 (b) Expansion ratio after storage at 60°C for 30 days.
[0067] Depend on Figure 5 (a) It can be seen that the capacity retention rate and recovery rate of scheme A (all LiPF6) are the largest, and the capacity retention rate and recovery rate of scheme F (all LiFSI) are the smallest, with a difference of 1.62% in retention rate and 0.91% in recovery rate.
[0068] Depend on Figure 5 (b) It can be seen that the expansion of scheme F (all LiFSI) is the largest, with an expansion rate of 6.26%, and the expansion of scheme A (all LiPF6) is the smallest, with an expansion rate of 2.25%. This shows that the high-temperature performance of all LiFSI is poor, which may be due to the fact that high temperature accelerates the corrosion of aluminum foil by all LiFSI.
[0069] Cycle performance test: Figure 6 (a) is the charge-discharge cycle curve at 25℃1C, Figure 6 (b) is the charge-discharge cycle curve at 45℃1C.
[0070] Depend on Figure 6 (a) It can be seen that after 2000 cycles at 25℃, the discharge capacity retention rates of schemes A, B, C, D, E, and F are not much different, which is consistent with Figure 5 This is consistent with the 25℃ discharge DCIR, indicating that the addition of LiFSI has little effect on the room temperature cycle.
[0071] As shown in Figure 6(b), after 1500 cycles at 45°C, the capacity retention rate of scheme F (full LiFSI) is the lowest, and it shows a rapid decay trend, which is consistent with the high-temperature storage test. This may be due to the fact that pure LiFSI has a certain degree of corrosion on the aluminum foil, which is related to the existence of the CS bond. The higher the temperature, the more obvious the corrosion.
[0072] SEM test of aluminum foil at the end of the cycle: Figure 7 (af) are SEM images of aluminum foil at the end of 45°C cycling.
[0073] Depend on Figure 7(af) It can be seen that the surface of the aluminum foil in Scheme A (all LiPF6) is smooth and has no holes. After adding LiFSI, certain holes appear on the surface of the electrode. The aluminum foil in Scheme F (all LiFSI) has more and larger holes, indicating that the corrosion of the aluminum foil by all LiFSI is the most serious, which is consistent with the results of high-temperature storage and high-temperature cycle tests.
[0074] The above-described embodiments are compared with the technical solutions and beneficial effects of the present invention, and it should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected.
Claims
1. A preparation method and application of an electrolyte containing LiFSI, characterized in that: The preparation method comprises: adding a mixed solvent, lithium hexafluorophosphate, and lithium bis(fluorosulfonyl)imide into a container in a glove box filled with argon gas, stirring and mixing, and obtaining an electrolyte containing LiFSI; The mass fraction of lithium bis(fluorosulfonyl)imide in the electrolyte is 2-10.5%, and the mass fraction of lithium hexafluorophosphate is 2-10.5%.
2. The method for preparing an electrolyte containing LiFSI according to claim 1, characterized in that: The total mass fraction of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide in the electrolyte is 14%.
3. The method for preparing an electrolyte containing LiFSI according to claim 1, characterized in that: The mixed solvent consists of ethylene carbonate, propylene carbonate, diethyl carbonate and dimethyl carbonate.
4. The method for preparing an electrolyte containing LiFSI according to claim 1, characterized in that: The mass ratio of ethylene carbonate, propylene carbonate, diethyl carbonate and dimethyl carbonate in the mixed solvent is 30:5:40:
25.
5. A lithium-ion battery having an electrolyte containing LiFSI obtained by the preparation method according to any one of claims 1 to 4, characterized in that: The lithium-ion battery consists of a positive electrode, a negative electrode, an electrolyte containing LiFSI, and a separator.
6. The lithium-ion battery containing the electrolyte of LiFSI according to claim 5, characterized in that: The positive electrode is lithium iron phosphate, the negative electrode is natural graphite, and the diaphragm is a PE diaphragm.
7. A method for preparing a lithium-ion battery containing an electrolyte containing LiFSI as claimed in claim 6, characterized in that: The preparation method comprises the following steps: die-cutting the positive electrode lithium iron phosphate and the negative electrode natural graphite respectively to make positive and negative electrode sheets, then laminating the positive and negative electrode sheets with PE diaphragms into soft-pack battery cells, and then welding, gluing, assembling, injecting electrolyte, forming, molding, and volume separation to obtain a lithium-ion battery.
Citation Information
Patent Citations
12V start-stop lithium ion battery electrolyte
CN112582674A
Electrolyte for low-temperature lithium ion battery electrolyte and lithium ion battery
CN112838272A
Lithium ion battery non-aqueous electrolyte and lithium ion battery
CN114142091A
4.5 V high-voltage ternary lithium ion battery electrolyte and preparation method and application thereof
CN116779970A
Lithium ion battery electrolyte with rate discharge at ultralow temperature and preparation method of lithium ion battery electrolyte
CN117728034A