Perovskite solar cell film packaging method and product

By preparing and encapsulating perovskite solar cell films in an oxygen-free environment and using Surlyn films for full coverage packaging, the stability of perovskite solar cell films in a photothermal environment is solved, and its stability and life are significantly improved. .

CN118984598APending Publication Date: 2024-11-19HUBEI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411064588.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The perovskite solar cell film has poor stability, especially in light and thermal environments, which leads to a short operating life.

Method used

Perovskite precursor solutions were prepared in an oxygen-free environment and films were coated under an oxygen-free conditions, followed by full coverage encapsulation using Surlyn films, optimizing the packaging temperature and time to ensure sealing and stability.

Benefits of technology

Effectively inhibit the degradation of perovskite solar cell films in photothermal environments, improve the stability and life of the film, and avoid the generation of volatile organic gases and material regeneration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984598A_ABST
    Figure CN118984598A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of solar energy, and particularly discloses a packaging method and a product of a perovskite solar cell thin film, and the packaging method comprises the steps: preparing a perovskite precursor solution in a water-free and oxygen-free environment, then coating the surface of a substrate with the perovskite precursor solution in the oxygen-free environment, and carrying out the packaging of the perovskite solar cell thin film. And finally, carrying out full-coverage packaging on the perovskite solar cell thin film by utilizing the Surlyn thin film in an oxygen-free environment. According to the invention, full-coverage packaging is carried out on the perovskite solar cell film by using the Surlyn film in an oxygen-free environment, degradation of the perovskite solar cell film when the perovskite solar cell film is stimulated by external high temperature and light can be effectively inhibited, volatile organic gas is generated, the regrowth process of the perovskite solar cell film is further inhibited, and the service life of the perovskite solar cell film is prolonged. Therefore, the problem of degradation of the perovskite solar cell in a photo-thermal environment is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of solar energy technology, and more specifically, to a packaging method and product of a perovskite solar cell film. Background Art

[0002] Perovskite solar cells (PSCs) based on organic-inorganic hybrid perovskites have become a low-cost, high-efficiency thin-film photovoltaic (PV) technology, and the power conversion efficiency (PCE) of PSCs has increased significantly from 9.7% in 2012 to 26.1%. The PCE of PSCs has now surpassed traditional thin-film solar technology, making it the most promising competitor to silicon-based solar cells.

[0003] The premise for the ultimate commercial application of new photovoltaic cells is to develop large-area modules with high efficiency, low cost and long-term stable operation. Compared with stability, the efficiency of large-area perovskite solar cells can be improved by improving the modular preparation process while deepening the understanding of the colloidal and solvent chemistry of perovskite solutions. In terms of service life, only a few research institutions have reported that the operational stability of PSCs will not decrease under 1000 hours of continuous illumination (there are very few with a retention rate of 100%, and the retention rate >95% is gradually increasing), and reports of illumination working stability reaching 10,000 hours are even rarer. In addition, the degradation of perovskites and devices may not be linear. When the damage of the material accumulates to a certain extent, a jump-like degradation may occur. Therefore, the stability of perovskite solar cell films needs to be further optimized. Summary of the invention

[0004] In view of the defects of the prior art, the present application provides a packaging method and product of a perovskite solar cell film, aiming to solve the problem of poor stability of the existing perovskite solar cell film.

[0005] According to one aspect of the present application, a method for encapsulating a perovskite solar cell thin film is provided, specifically comprising:

[0006] S1 prepares the perovskite precursor solution in an anhydrous and oxygen-free environment;

[0007] S2 coating the perovskite precursor solution on the surface of the substrate in an oxygen-free environment to form a uniformly dispersed perovskite solar cell film;

[0008] S3 uses a Surlyn film to fully cover and encapsulate the perovskite solar cell film in an oxygen-free environment, thereby achieving encapsulation of the perovskite solar cell film.

[0009] Compared with the prior art, the above technical solution conceived by the present application can effectively inhibit the degradation of the perovskite solar cell film and improve the stability of the perovskite solar cell film, because the present application proposes to use Surlyn film to fully cover the perovskite solar cell film in an oxygen-free environment.

[0010] As a further preferred embodiment, the solute of the perovskite precursor solution is Cs 0.05 (FA 0.85 MA 0.15 ) 0.95 Pb(Br 0.15 I 0.85 )3, FAPbI3 or FA 0.9 Cs 0.1 PbI.

[0011] As further preferred, step S1 specifically comprises: weighing the raw materials in an anhydrous and oxygen-free environment according to the stoichiometric ratio of the solute, and then dissolving the weighed raw materials in a polar solvent to prepare a perovskite precursor solution.

[0012] As further preferred, the polar solvent is a mixed solution of dimethyl sulfoxide and N,N-dimethylformamide.

[0013] As further preferred, in step S2, the substrate is FTO glass, ITO glass or a flexible ITO conductive substrate.

[0014] As further preferred, in step S2, the substrate is cleaned and treated with an ultraviolet ozone machine before coating the perovskite precursor solution.

[0015] As further preferred, in step S2, the perovskite precursor solution is coated by a two-step spin coating method, wherein the rotation speed in the first step of spin coating is 1000rpm-2000rpm, and the spin coating time is 6s-10s; the rotation speed in the second step of spin coating is 4000rpm-5000rpm, and the spin coating time is 20s-25s.

[0016] As further preferred, in step S2, after the coating of the perovskite precursor solution is completed, anti-solvent chlorobenzene is dripped onto the substrate, and thermal annealing is performed at a temperature of 140° C. to 150° C. for 10 min to 15 min to obtain a black mirror-like perovskite solar cell film.

[0017] As a further preferred embodiment, step S3 is specifically as follows: placing a Surlyn film on the surface of the perovskite solar cell film, then covering it with a glass sheet and keeping it at 100°C to 120°C for 2min to 3min, so as to achieve the encapsulation of the perovskite solar cell film.

[0018] According to another aspect of the present application, a tightly encapsulated perovskite solar cell film prepared by the above encapsulation method is provided.

[0019] In general, the above technical solutions conceived by this application have the following technical advantages compared with the prior art:

[0020] 1. This application proposes to use Surlyn film to fully cover and encapsulate the perovskite solar cell film in an oxygen-free environment, which can effectively inhibit the degradation of the perovskite solar cell film when it is stimulated by external high temperature and light, generate volatile organic gas, and then inhibit the regrowth process of the perovskite solar cell film, thereby solving the problem of degradation of perovskite solar cells in a photothermal environment;

[0021] 2. In particular, the present application optimizes the Surlyn film packaging temperature and packaging time, which can ensure the sealing of the packaging while avoiding the decomposition of the MA group and the FA group. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a packaging flow chart of a perovskite solar cell thin film provided in an embodiment of the present application;

[0023] Figure 2 These are scanning electron microscope morphology images of the perovskite solar cell thin films obtained in Example 1, Comparative Examples 1 and 2 of the present application after aging under the conditions of light, high temperature and dual external pressure, wherein (a) is Example 1, (b) is Comparative Example 1, and (c) is Comparative Example 2;

[0024] Figure 3 The XRD spectra of the perovskite solar cell films obtained in Example 1 and Comparative Examples 1 and 2 of the present application after aging under the conditions of light, high temperature and dual external pressure;

[0025] Figure 4 It is a UV-visible light absorption spectrum diagram of the perovskite solar cell film obtained in Example 1 and Comparative Examples 1 and 2 of the present application after aging under the conditions of light, high temperature and dual external pressure;

[0026] Figure 5 It is a steady-state photoluminescence spectrum diagram of the perovskite solar cell film obtained in Example 1 and Comparative Examples 1 and 2 of the present application after aging under dual external pressure conditions of light and high temperature. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0028] like Figure 1 As shown, the present application provides a packaging method for a perovskite solar cell thin film, specifically:

[0029] S1 prepares perovskite precursor solution based on highly volatile polar solvent in an anhydrous and oxygen-free environment;

[0030] S2 applies the perovskite precursor solution to the surface of the substrate in an oxygen-free environment to form a uniformly dispersed perovskite solar cell film;

[0031] S3 uses Surlyn film to fully cover and encapsulate the perovskite solar cell film in an oxygen-free environment, thereby achieving the encapsulation of the perovskite solar cell film.

[0032] The present application proposes to use Surlyn film to fully cover and encapsulate the perovskite solar cell film in an oxygen-free environment, which can effectively inhibit the degradation of the perovskite solar cell film and improve the stability of the perovskite solar cell film.

[0033] Furthermore, the solute of the perovskite precursor solution is Cs 0.05 (FA 0.85 MA 0.15 ) 0.95 Pb(Br 0.15 I 0.85 )3, FAPbI3 or FA 0.9 Cs 0.1 When preparing the perovskite precursor solution, the raw material is first accurately weighed according to the stoichiometric ratio of the solute in an anhydrous and oxygen-free environment, and then dissolved in a highly volatile polar solvent formed by a mixture of dimethyl sulfoxide and N,N-dimethylformamide, and stirred evenly for 4h to 5h to obtain the perovskite precursor solution.

[0034] Further, in step S2, the substrate is FTO glass, ITO glass or flexible ITO conductive substrate that has been cleaned and treated by an ultraviolet sampling machine, and the substrate is ultrasonically cleaned with deionized water, acetone, isopropanol and ethanol for 20 minutes to 30 minutes, and treated with ultraviolet irradiation for 20 minutes to 40 minutes.

[0035] Furthermore, in step S2, a two-step spin coating method is used to coat the perovskite precursor solution, wherein the first step of the spin coating has a rotation speed of 1000 rpm to 2000 rpm and a spin coating time of 6 s to 10 s; the second step of the spin coating has a rotation speed of 4000 rpm to 5000 rpm and a spin coating time of 20 s to 25 s. Too fast a spin coating speed will result in uneven spin coating of the perovskite precursor solution on the glass substrate; too short a spin coating time will result in the inability to spin coat the anti-solvent at the appropriate time, resulting in poor crystallinity of the film; too long a spin coating time will result in the failure to perform the annealing post-treatment process at the appropriate time, causing the solvent in the film to volatilize by itself, resulting in weakened perovskite crystallinity and poor quality of the perovskite film.

[0036] Further, in step S2, after the coating of the perovskite precursor solution is completed, the anti-solvent chlorobenzene is dripped onto the substrate, and thermal annealing is performed at a temperature of 140°C to 150°C for 10min to 15min, thereby obtaining a black mirror perovskite solar cell film. If the annealing temperature is too low, the perovskite film cannot be transformed into a photoactive phase, and the longer annealing time corresponds to, the greater the possibility of film decomposition; if the annealing temperature is too high, the decomposition of the perovskite film will be aggravated, and the quality of the perovskite film will be reduced.

[0037] Further, step S3 is specifically as follows: cut a Surlyn film of the same size as the substrate and place it on the surface of the perovskite solar cell film, then cover it with a thin white glass sheet, clamp it with pressure and place it at 100℃~120℃ for 2min~3min, so as to realize the encapsulation of the perovskite solar cell film. When the encapsulation temperature is low, small bubbles are easily generated when the Surlyn film is heated and softened, and it is impossible to complete uniform bonding, which weakens the air tightness of the encapsulation. When the temperature is low, the heating process is longer, and the MA-related components in the perovskite film are prone to decomposition when heated for a long time in the range of 65℃~85℃; at the same time, considering that even if the FA-based perovskite film has good thermal stability in the range of 85℃~150℃, long-term high temperature will also cause irreversible degradation to the perovskite solar cell itself, so the temperature cannot be too high, and the insulation time is controlled at 2min~3min.

[0038] Furthermore, the entire process was handled in an inert atmosphere of N2, the perovskite solar cell film was prepared in a glove box, and the film encapsulation was performed in the glove box.

[0039] According to another aspect of the present application, a tightly encapsulated perovskite solar cell film prepared by the above encapsulation method is provided, and the perovskite solar cell film can still maintain good film morphology and photoelectric properties after being irradiated with a high temperature of 85°C and AM1.5 sunlight.

[0040] The technical solution provided in this application is further described below based on specific embodiments.

[0041] Example 1

[0042] S1 In an anhydrous and oxygen-free environment, the perovskite precursors including lead iodide, lead bromide, methylamine bromide, iodomethane, and cesium iodide are prepared according to (Cs 0.05 (FA 0.85 MA 0.15 ) 0.95 Pb(Br 0.15 I 0.85 )3) The stoichiometric ratio is accurately weighed, and then N, N-dimethylformamide and dimethyl sulfoxide solution are added as solvents in a volume ratio of 4:1, and a perovskite precursor solution is obtained after magnetic stirring for 4 hours;

[0043] S2: coating a liquid perovskite precursor solution on the surface of a substrate, and performing thermal annealing at 150°C for 10 minutes to obtain a light-absorbing layer film of a solar cell with a black mirror surface. The spin coating includes two steps: spin coating at a speed of 1000 rpm for 10 seconds, spin coating at a speed of 4000 rpm for 20 seconds, and dropping 200 microliters of chlorobenzene onto the rotating perovskite film at the last second of the second stage of spin coating. The substrate is selected from FTO glass. The substrate is sequentially ultrasonically cleaned with deionized water, acetone, isopropanol, and ethanol for 20 minutes to 30 minutes, and subjected to ultraviolet irradiation for 20 minutes to 40 minutes.

[0044] S3 cut a Surlyn film of the same size as the above substrate in a water-free and oxygen-free environment and place it on the surface of the perovskite solar cell film, cover it with a thin white glass sheet, clamp it with a pressure clamp and place it in a constant temperature box at 120°C for 2 minutes to complete the packaging.

[0045] Example 2

[0046] S1 In an anhydrous and oxygen-free environment, the perovskite precursors including lead iodide, lead bromide, methylamine bromide, iodomethane, and cesium iodide are prepared according to (Cs 0.05 (FA 0.85 MA 0.15 ) 0.95 Pb(Br 0.15 I 0.85 )3) The stoichiometric ratio is accurately weighed, and then N, N-dimethylformamide and dimethyl sulfoxide solution are added as solvents in a volume ratio of 4:1, and a perovskite precursor solution is obtained after magnetic stirring for 4 hours;

[0047] S2: coating a liquid perovskite precursor solution on the surface of a substrate, and performing thermal annealing at 140°C for 10 minutes to obtain a light-absorbing layer film of a solar cell with a black mirror surface. The spin coating includes two steps: spin coating at a speed of 1500 rpm for 8 seconds, spin coating at a speed of 5000 rpm for 20 seconds, and dropping 200 microliters of chlorobenzene onto the rotating perovskite film at the last second of the second stage of spin coating. The substrate is selected from FTO glass. The substrate is sequentially ultrasonically cleaned with deionized water, acetone, isopropanol, and ethanol for 20 minutes to 30 minutes, and subjected to ultraviolet irradiation for 20 minutes to 40 minutes.

[0048] S3 cuts a Surlyn film of the same size as the above substrate in a water-free and oxygen-free environment and places it on the surface of the perovskite solar cell film. It is covered with a thin white glass sheet, clamped with a pressure clamp, and placed in a constant temperature box at 100°C for 3 minutes to complete the packaging.

[0049] Example 3

[0050] S1 In an anhydrous and oxygen-free environment, the perovskite precursors including FAI and PbI2 are accurately weighed according to the stoichiometric ratio of FAPbI3, and then N, N-dimethylformamide and dimethyl sulfoxide solution are added as solvents in a volume ratio of 4:1, and the perovskite precursor solution is obtained after magnetic stirring for 4 hours;

[0051] S2: coating a liquid perovskite precursor solution on the surface of a substrate, and performing thermal annealing at 145°C for 15 minutes to obtain a light-absorbing layer film of a solar cell with a black mirror surface. The spin coating includes two steps: spin coating at a speed of 2000 rpm for 6 seconds, spin coating at a speed of 4500 rpm for 25 seconds, and dropping 200 microliters of chlorobenzene onto the rotating perovskite film at the last second of the second stage of spin coating. The substrate is selected from FTO glass. The substrate is sequentially ultrasonically cleaned with deionized water, acetone, isopropanol, and ethanol for 20 minutes to 30 minutes, and subjected to ultraviolet irradiation for 20 minutes to 40 minutes.

[0052] S3 cuts a Surlyn film of the same size as the above substrate in a water-free and oxygen-free environment and places it on the surface of the perovskite solar cell film. It is covered with a thin white glass sheet, clamped with a pressure clamp, and placed in a constant temperature box at 110°C for 2.5 minutes to complete the packaging.

[0053] Example 4

[0054] S1 In an anhydrous and oxygen-free environment, the perovskite precursors including CsI, FAI, and PbI2 are prepared according to FA 0.9 Cs 0.1 The stoichiometric ratio of PbI3 was accurately weighed, and then N, N-dimethylformamide and dimethyl sulfoxide solution were added as solvents in a volume ratio of 4:1, and the perovskite precursor solution was obtained after magnetic stirring for 4 h;

[0055] S2 coats the liquid perovskite precursor solution on the surface of the substrate and performs thermal annealing at 140 °C for 13 min to obtain a light-absorbing layer film of a black mirror-like solar cell. The spin coating includes two steps, spin coating at a speed of 1800 rpm for 9 s, spin coating at a speed of 4200 rpm for 22 s, and dropping 200 μl of chlorobenzene onto the rotating perovskite film in the last second of the second-stage spin coating. The substrate is selected from FTO glass. The substrate is ultrasonically cleaned with deionized water, acetone, isopropanol, and ethanol for 20 min to 30 min in sequence and is treated with ultraviolet irradiation for 20 min to 40 min;

[0056] S3 In an anhydrous and oxygen-free environment, cut a Surlyn film of the same size as the above substrate and place it on the surface of the perovskite solar cell film, cover it with a thin white glass sheet, clamp it with a pressure clamp, and place it in an incubator at 105 °C for 2 min to complete the encapsulation.

[0057] Comparative Example 1

[0058] S1 In an anhydrous and oxygen-free environment, weigh accurately the perovskite precursors including lead iodide, lead bromide, bromomethylamine, iodomethylformamidine, and cesium iodide according to the stoichiometric ratio of (Cs 0.05 (FA 0.85 MA 0.15 ) 0.95 Pb(Br 0.15 I 0.85 )3), then add N,N-dimethylformamide and dimethyl sulfoxide solution as solvents according to a volume ratio of 4:1, and obtain a perovskite precursor solution after magnetic stirring for 4 h;

[0059] S2 coats the liquid perovskite precursor solution on the surface of the substrate and performs thermal annealing at 150 °C for 10 min to obtain a light-absorbing layer film of a black mirror-like solar cell. The spin coating includes two steps, spin coating at a speed of 1000 rpm for 10 s, spin coating at a speed of 4000 rpm for 20 s, and dropping 200 μl of chlorobenzene onto the rotating perovskite film in the last second of the second-stage spin coating. The substrate is selected from FTO glass, ITO glass, and flexible ITO conductive substrate. The substrate is ultrasonically cleaned with deionized water, acetone, isopropanol, and ethanol for 20 min to 30 min in sequence and is treated with ultraviolet irradiation for 20 min to 40 min;

[0060] S3 In an anhydrous and oxygen-free environment, cut a Surlyn film in a "hui" character shape and place it on the surface of the perovskite solar cell film, cover it with a thin white glass sheet, clamp it with a pressure clamp, and place it in an incubator at 130 °C for 2 - 3 min to obtain an incompletely sealed perovskite solar cell film.

[0061] Comparative Example 2

[0062] S1 In an anhydrous and oxygen-free environment, the perovskite precursors including lead iodide, lead bromide, methylamine bromide, iodomethane, and cesium iodide are prepared according to (Cs 0.05 (FA 0.85 MA 0.15 ) 0.95 Pb(Br 0.15 I 0.85 )3) The stoichiometric ratio is accurately weighed, and then N, N-dimethylformamide and dimethyl sulfoxide solution are added as solvents in a volume ratio of 4:1, and a perovskite precursor solution is obtained after magnetic stirring for 4 hours;

[0063] S2 coats the liquid perovskite precursor solution on the surface of the substrate and performs thermal annealing at 150°C for 10 minutes to obtain a black mirror-like light-absorbing layer film of the solar cell. The spin coating includes two steps, spin coating at a speed of 1000 rpm for 10 seconds and spin coating at a speed of 4000 rpm for 20 seconds, and in the last second of the second stage of spin coating, 200 microliters of chlorobenzene is dropped onto the rotating perovskite film. The substrate is selected from FTO glass, ITO glass and flexible ITO conductive substrate. The substrate is ultrasonically cleaned with deionized water, acetone, isopropanol and ethanol for 20 minutes to 30 minutes, and is treated with ultraviolet irradiation for 20 minutes to 40 minutes to obtain an unencapsulated perovskite solar cell film.

[0064] The tightly encapsulated perovskite solar cell film prepared in Example 1, the non-tightly encapsulated perovskite solar cell film prepared in Comparative Example 1, and the non-encapsulated perovskite solar cell film prepared in Comparative Example 2 were placed under dual external pressure conditions of high temperature (AM1.5, 1 sun; 85°C) for aging.

[0065] Figure 2 (b) and (c) are scanning electron microscope cross-sectional morphology images of the perovskite solar cell film in Comparative Examples 1 and 2 after aging under dual external pressure conditions of light and high temperature (AM1.5, 1 sun; 85°C). Figure 2 It can be seen that holes appeared in the unencapsulated film after exposure to light, and the number of holes in the film after aging under the dual conditions of high temperature and light increased significantly and the film thickness decreased; in the case of not tightly encapsulated, after light immersion, perovskite regrowth occurred on the perovskite solar cell film; Figure 1 (a) is the tightly packaged film in Example 1. It can be seen that the film is almost not degraded and no "coral-like" substance is generated.

[0066] Figure 3They are respectively the XRD patterns of the perovskite solar cell film aged under dual external pressure conditions of high temperature (AM1.5, 1 sun; 85°C) under illumination in Example 1 and Comparative Examples 1 and 2, wherein Fresh is the XRD of the tightly encapsulated perovskite solar cell film obtained in Example 1 without being aged under illumination, HLS24h@w Hermetic is the XRD of the tightly encapsulated perovskite solar cell film obtained in Example 1 after being aged under illumination for 24 hours, HLS24h@w / o Hermetic is the XRD of the non-tightly encapsulated perovskite solar cell film obtained in Comparative Example 1 after being aged under illumination for 24 hours, and HLS 8h@No sealing is the XRD of the non-encapsulated perovskite solar cell film obtained in Comparative Example 2 after being aged under illumination for 8 hours. Figure 2 It can be seen that the unencapsulated film in Comparative Example 2 has been severely degraded within 8 hours, the peak intensity of the photoactive phase of α-FAPbI3 has dropped sharply, and the non-photoactive yellow phase of δ-FAPbI3 has appeared; under the same aging conditions, the film in Example 1 still has good crystallinity after aging for 24 hours, but the peak intensity of the photoactive phase of α-FAPbI3 has slightly decreased, and the peak intensity of the characteristic peak of the PbI2 (001) crystal plane has increased; and although the film in Comparative Example 1 that is not tightly encapsulated is slower than the film in Comparative Example 2, its photoactive peak intensity has been significantly reduced. This shows that the degradation of the perovskite solar cell film in a photothermal environment can be effectively suppressed after being encapsulated by Surlyn film.

[0067] Figure 4 They are respectively the UV-visible absorption spectra of the perovskite solar cell thin film after aging under the dual external pressure conditions of light and high temperature (AM1.5, 1 sun; 85°C) in Example 1 and Comparative Examples 1 and 2, and the annotations are as shown above. Figure 3 It can be seen that the absorbance of the film in Example 1 is slightly lower than that of the original film after aging for 24 hours under the double aging conditions, indicating that the film is partially degraded, while the absorbance of the film in Comparative Example 1 is greatly reduced after aging for 24 hours, but it is still stronger than that of the film in Comparative Example 2. This shows that the degradation of the perovskite solar cell film in a light-heat environment can be effectively suppressed after encapsulation by Surlyn film.

[0068] Figure 5 They are steady-state photoluminescence spectra of the perovskite solar cell thin film after aging under dual external pressure conditions of high temperature (AM1.5, 1 sun; 85°C) in Example 1 and Comparative Examples 1 and 2, respectively, and the annotations are as shown above. Figure 4It can be seen that after 24 hours of dual-condition aging, the photoluminescence intensity of the perovskite solar cell film in Example 1 is slightly reduced, and the peak position is almost unchanged, indicating that the components are slightly degraded; the film intensity in Comparative Example 1 is reduced and the peak position is red-shifted, and the unencapsulated film in Comparative Example 2 has a weak absorption peak at around 650nm, which is consistent with the UV test, indicating that the surface of the tightly encapsulated film has fewer defects and less non-radiative recombination after aging. It further illustrates that the degradation of the perovskite solar cell film in a light-heat environment can be effectively suppressed after encapsulation by Surlyn film.

[0069] The experiment shows that the Surlyn film has an encapsulation effect on the perovskite solar cell film. After the unencapsulated perovskite solar cell film is aged under the dual external pressure conditions of light and high temperature (AM1.5, 1 sun; 85°C), a large number of holes appear in the film, so that the film collapses; after the untightly encapsulated perovskite solar cell film is aged under the dual external pressure conditions of light and high temperature (AM1.5, 1 sun; 85°C), the film does not have holes, but the film has a regrowth process; under the same conditions, the tightly encapsulated perovskite solar cell film still has good uniformity and relatively good photoelectric performance. In addition, after the solar cell device structure is encapsulated accordingly, the solar cell life test results show that the stability of the encapsulated solar cell is greatly improved compared with the unencapsulated device; and the stability of the tightly encapsulated solar cell device is better than that of the unencapsulated device. This application uses the Surlyn film to tightly encapsulate the perovskite solar cell film, inhibit the regrowth process of the perovskite solar cell film in the light and heat environment, further reduce the degradation of the perovskite solar cell film and the solar cell device, and provide a new idea for improving the stability of the perovskite solar cell.

[0070] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A method for encapsulating a perovskite solar cell thin film, characterized in that: The packaging method is specifically as follows: S1 prepares the perovskite precursor solution in an anhydrous and oxygen-free environment; S2 coating the perovskite precursor solution on the surface of the substrate in an oxygen-free environment to form a uniformly dispersed perovskite solar cell film; S3 uses a Surlyn film to fully cover and encapsulate the perovskite solar cell film in an oxygen-free environment, thereby achieving encapsulation of the perovskite solar cell film.

2. The packaging method according to claim 1, characterized in that: The solute of the perovskite precursor solution is Cs 0.05 (FA 0.85 MA 0.15 ) 0.95 Pb(Br 0.15 I 0.85 )3, FAPbI3 or FA 0.9 Cs 0.1 PbI3.

3. The packaging method according to claim 2, characterized in that: Step S1 specifically includes: weighing the raw materials in an anhydrous and oxygen-free environment according to the stoichiometric ratio of the solute, and then dissolving the weighed raw materials in a polar solvent to prepare a perovskite precursor solution.

4. The packaging method according to claim 3, characterized in that: The polar solvent is a mixed solution of dimethyl sulfoxide and N,N-dimethylformamide.

5. The packaging method according to claim 1, characterized in that: In step S2, the substrate is FTO glass, ITO glass or a flexible ITO conductive substrate.

6. The packaging method according to claim 1, characterized in that: In step S2, the substrate is cleaned and treated with an ultraviolet ozone machine before coating the perovskite precursor solution.

7. The packaging method according to claim 1, characterized in that: In step S2, the perovskite precursor solution is coated by a two-step spin coating method. In the first step of spin coating, the rotation speed is 1000rpm~2000rpm, and the spin coating time is 6s~10s; in the second step of spin coating, the rotation speed is 4000rpm~5000rpm, and the spin coating time is 20s~25s.

8. The packaging method according to claim 1, characterized in that: In step S2, after the coating of the perovskite precursor solution is completed, anti-solvent chlorobenzene is added dropwise on the substrate, and thermal annealing is performed at a temperature of 140° C. to 150° C. for 10 min to 15 min to obtain a black mirror perovskite solar cell film.

9. The packaging method according to any one of claims 1 to 8, characterized in that: Step S3 is specifically as follows: placing a Surlyn film on the surface of the perovskite solar cell film, then covering it with a glass sheet and keeping it at 100° C. to 120° C. for 2 min to 3 min, so as to achieve the encapsulation of the perovskite solar cell film.

10. A tightly encapsulated perovskite solar cell film prepared by the encapsulation method according to any one of claims 1 to 9.