Method for producing polymer solution

Through two concentration steps and prepolymer solution preparation method, the problems of low preparation efficiency of resist polymer solution and insufficient removal of impurities in the prior art are solved, and efficient and uniform preparation of high polymer concentration solutions are achieved. For thick film applications.

CN118984850APending Publication Date: 2024-11-19MARUZEN PETROCHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380026777.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-18
Filing Date
2023-04-17
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently manufacture resist polymer solutions with high polymer concentration and desired ratios, especially in thick film applications, where higher polymer concentration and viscosity lead to low preparation efficiency and insufficient removal of impurities, which affects Product quality.

Method used

Two concentration steps and prepolymer solution preparation method are adopted to adjust the solvent composition and concentration to achieve accurate control of polymer concentration and solvent replacement, ensuring efficient preparation of polymer solution.

Benefits of technology

It is achieved efficiently manufacturing of resist polymer solutions with high polymer concentration and desired ratios, suitable for thick film applications, improves preparation efficiency and product quality, and ensures polymer uniformity and high purity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005036659850000061
    Figure BDA0005036659850000061
  • Figure BDA0005036659850000071
    Figure BDA0005036659850000071
  • Figure BDA0005036659850000081
    Figure BDA0005036659850000081
Patent Text Reader

Abstract

Provided is a method capable of efficiently mass-producing a polymer solution having a high polymer concentration and containing a plurality of solvents at a desired ratio, said polymer solution being useful in the preparation of a resist composition for thick films. The present invention is a method for producing a polymer solution in which C mass% of a polymer is contained in a mixed solvent obtained by mixing at least two solvents at a predetermined mass ratio, the polymer concentration and solvent composition of a "prepolymer solution" are estimated such that the solvent composition becomes just a prescribed value even when the polymer solution containing all of the solvent is concentrated to a target concentration C mass%, and a target polymer solution is produced by concentrating the prepolymer solution after the prepolymer solution is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a polymer solution containing two or more solvents. More specifically, the present invention relates to a method for producing a polymer solution containing two or more solvents useful for preparing a resist composition. Background Art

[0002] In the manufacture of semiconductors, ultra-fine processing with a line width of less than 10nm has become a cutting-edge technology, and on the other hand, three-dimensional processing technologies such as 3D-NAND are also developing. In three-dimensional processing, a resist film with a thickness of several microns to tens of microns is required, and the resist composition used therefor requires a corresponding resist resin concentration and viscosity.

[0003] On the other hand, in order to improve the pattern shape or improve the coating properties, there are many examples of using mixed solvents to prepare resist compositions. For example, in Patent Document 1, a resin composition useful for thick film resists, which contains a solvent with a viscosity and a boiling point within a specific range, is disclosed. Specifically, a resin composition is exemplified, which is obtained by dissolving a copolymer of para-hydroxystyrene and tert-butyl methacrylate, an acid generator and other additives in various mixed solvents such as propylene glycol monomethyl ether acetate / ethyl acetate, propylene glycol monomethyl ether / cyclohexanone. In Patent Document 2, a thick film photoresist composition is disclosed, which contains more than 40% by mass of an organic solvent having a boiling point of more than 150°C at atmospheric pressure and a contact angle of less than 18 degrees with a silicon substrate in all organic solvents. Specifically, a resist composition having a polymer concentration of 49.5% by mass is disclosed, wherein a polymer, an alkali-soluble polymer, an acid generator, and an acid diffusion control agent that can increase solubility in an alkali by the action of an acid are dissolved in a mixed solvent of propylene glycol monomethyl ether acetate and 3-methoxybutyl acetate. In addition, in patent documentation 3, a resist dry film obtained by coating the following resist composition in a PET film-like manner is disclosed, wherein the resist composition is obtained by dissolving a copolymer of hydroxystyrene and amyloxystyrene and an acid generator in a mixed solvent of propylene glycol monomethyl ether acetate and propylene glycol or a mixed solvent of propylene glycol monomethyl ether acetate and cyclopentanone at a polymer concentration of about 50% by mass. These resist compositions are all prepared by mixing a solid polymer with an acid generator and other additives and dissolving them in a solvent. The method is easy to adjust the concentration of each component, but on the other hand, the polymer must be fully dried in a manner such that the polymerization solvent, purification solvent, etc. used when manufacturing the polymer will not remain in the solid polymer as impurities. However, there is a concern about the decomposition and denaturation of resist polymers caused by heat, so it is not easy to highly dry a large amount of polymers in industrial production from the perspective of equipment and process time. In addition, in order to dissolve a large amount of solid polymers in a solvent again and make a uniform solution, it also takes a lot of time, which becomes the main reason for increasing manufacturing costs.

[0004] Therefore, the following method is implemented: when manufacturing a polymer, the polymer is not made into a dry solid but refined into a polymer solution, and an acid generator, an additive and a solvent are mixed and dissolved therein to prepare a resist composition. As a method for preparing a polymer solution, the following method is disclosed in Patent Document 4: after the polymer solution after the polymerization reaction is precipitated and purified, the polymer is redissolved in a solvent having a boiling point lower than that of the solvent used for the resist composition, and the low boiling point solvent is distilled off by reduced pressure distillation while adding a resist solvent to replace the solvent of the polymer solution with a resist solvent. Specifically, in Patent Document 4, after the polymerization of the ArF resist polymer, water washing, filtration, precipitation purification and rinsing operations are performed, and the obtained wet polymer is dissolved in a mixed solvent of propylene glycol monomethyl ether acetate and propylene glycol monomethyl ether, and it is concentrated, thereby preparing a polymer solution for photoresist with a polymer concentration of 25% by weight. In addition, in Patent Documents 5 and 6, a method for preparing a polymer solution for photoresist containing multiple solvents is disclosed. Specifically, in Patent Document 5, after obtaining a polymer containing at least repeating units including a group that can become alkali-soluble by the action of an acid and repeating units including an alicyclic skeleton having a polar group by polymerization, precipitation purification is carried out, and the separated wet polymer is dissolved in propylene glycol monomethyl ether. After removing the low-boiling point components by distillation, propylene glycol monomethyl ether acetate and propylene glycol monomethyl ether are added to adjust the polymer concentration to 20% by weight to prepare a polymer solution for photoresist (PGMEA / PGME weight ratio = 7 / 3).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2018 / 061512

[0008] Patent Document 2: Japanese Patent Application Publication No. 2014-127518

[0009] Patent Document 3: Japanese Patent Application Publication No. 2019-105847

[0010] Patent Document 4: Japanese Patent Application Publication No. 2005-173252

[0011] Patent Document 5: Japanese Patent Application Publication No. 2006-161052

[0012] Patent Document 6: Japanese Patent Application Publication No. 2006-176574 Summary of the invention

[0013] Problems to be solved by the invention

[0014] However, the method of patent document 4 must be fully distilled and removed by the process of concentration in a manner that the solvent (impurities) used in the precipitation purification and rinsing operation will not be mixed, but at the time point when the concentration reaches the target polymer concentration, the removal of the aforementioned impurities may not be sufficient. In addition, since the vapor pressure of propylene glycol monomethyl ether acetate is different from that of propylene glycol monomethyl ether, the speed of distillation removal is different when concentrated, and there is also a worry that the composition of the mixed solvent after concentration will not become the desired value. On the other hand, with regard to the method of patent document 5, another solvent is added after the polymer solution of a solvent in the mixed solvent is concentrated, so it is easy to remove impurities and adjust the polymer concentration and the composition of the mixed solvent, but it is not suitable for preparing a polymer solution with a higher polymer concentration. For example, it is assumed that the composition weight ratio of 2 mixed solvents is 1:1 and the polymer concentration is 60% by mass. In the case of a polymer solution, it is necessary to add another solvent 2 parts by mass and stir and homogenize after at least concentrating to a polymer concentration of 75% by mass (6 parts by mass of polymer: 2 parts by mass of solvent), but at such a high concentration, the possibility of polymer precipitation in large quantities or being unable to stir due to high viscosity becomes high.

[0015] The polymer concentration and viscosity of resist compositions for thick films tend to be high, and accordingly, the polymer solution before adding an acid generator or an additive tends to require a high polymer concentration. A method for efficiently producing a polymer solution having a high polymer concentration and containing a mixed solvent is required.

[0016] Therefore, an object of the present invention is to provide a method for efficiently producing a polymer solution having a high polymer concentration and containing a plurality of solvents at a desired ratio, the polymer solution being suitable for preparing a resist composition, particularly a resist composition for thick films.

[0017] Means for solving problems

[0018] The inventors of the present application have conducted intensive research and found that the above-mentioned problems can be solved by sequentially carrying out the first concentration step, the prepolymer solution preparation step and the second concentration step described in detail below in a method for producing a polymer solution containing a polymer in a mixed solvent obtained by mixing at least two or more solvents in a specified mass ratio.

[0019] That is, according to the present invention, the following inventions can be provided.

[0020] [1] A method for producing a polymer solution, characterized in that the method comprises producing a polymer solution containing C mass % of a polymer in a mixed solvent obtained by mixing at least two or more solvents at a predetermined mass ratio,

[0021] The manufacturing method comprises the following steps:

[0022] First concentration step: A step of concentrating a solution obtained by dissolving the aforementioned polymer in at least one of the solvents in the aforementioned mixed solvent so that the polymer concentration becomes Cz (0.8C < Cz ≤ C + 10) mass%;

[0023] Prepolymer solution preparation step: A step of preparing a prepolymer solution by adding a solvent for the mixed solvent to the polymer solution obtained in the aforementioned first concentration step. In this step,

[0024] the aforementioned prepolymer solution is a solution containing a polymer at a concentration Ck (0.3C ≤ Ck ≤ 0.8C) mass% in the aforementioned mixed solvent, and is a solution in which when the aforementioned prepolymer solution is concentrated from a polymer concentration of Ck mass% to C mass%, the mass ratio of at least two or more solvents in the aforementioned mixed solvent becomes ±5% of the aforementioned specified mass ratio; and

[0025] Second concentration step: A step of concentrating the aforementioned prepolymer solution to a polymer concentration of C mass%.

[0026] [2] The method for manufacturing a polymer solution as described in [1], wherein the mass ratio of each solvent in the aforementioned prepolymer solution is obtained through the following preliminary test.

[0027] (Steps of the preliminary test)

[0028] Set the polymer concentration Ck of the prepolymer solution. Calculate the concentration degree R of the solvent when the prepolymer solution is concentrated in the second concentration step {R = (100 - C) / (100 × C / Ck - C)}.

[0029] Next, prepare a mixed solvent in which the composition of the solvent that is considered to be largely distilled off during distillation according to the boiling point and vapor pressure of each solvent is more than the target composition, perform distillation until the total mass of the mixed solvent is reduced to the value obtained by multiplying it by the concentration degree R, and obtain the solvent composition ratio after distillation. Obtain the mixed solvent composition ratio at which the solvent composition ratio after distillation becomes equal to the target composition, and use this mixed solvent composition ratio as the mass ratio of each solvent in the prepolymer solution.

[0030] [3] The method for manufacturing a polymer solution as described in [1] or [2], wherein a solvent replacement step is further included before the first concentration step: a step of reducing low-boiling impurities other than this solvent by performing distillation under reduced pressure while adding at least one of the solvents in the aforementioned mixed solvent to the solution containing the aforementioned polymer.

[0031] [4] The method for producing a polymer solution according to any one of [1] to [3], further comprising, after the second concentration step, a component adjustment step of adding a solvent to the polymer solution to adjust the polymer concentration and the composition of the mixed solvent.

[0032] [5] The method for producing a polymer solution according to any one of [1] to [4], wherein the polymer concentration C in the polymer solution is 30 to 70% by mass.

[0033] [6] A method for producing a polymer solution as described in any one of [1] to [5], wherein the concentration of the first solvent is 45% by mass or more and less than 80% by mass, and the concentration of the second solvent is 20% by mass or more and less than 50% by mass, relative to the total mass of the mixed solvent of the aforementioned polymer solution.

[0034] [7] The method for producing a polymer solution according to any one of [1] to [6], wherein the polymer is a resist polymer and the mixed solvent is a resist solvent.

[0035] Effects of the Invention

[0036] According to the present invention, a polymer solution having a high polymer concentration and containing a plurality of solvents at a desired ratio, which is suitable for preparing a resist composition, particularly a resist composition for a thick film, can be efficiently produced on a commercial scale. DETAILED DESCRIPTION

[0037] [polymer]

[0038] The type of polymer applicable to the present invention is not limited, but the present invention is suitable for efficiently producing a resist polymer solution useful in the preparation of a photoresist composition, and any polymer known in the art for resists can be applied without particular limitation. In the present invention, as the polymer, the resist polymer described in detail below is preferably used.

[0039] [Polymer for resist]

[0040] The polymer for resist is a polymer whose solubility in a developer can be changed by the action of an acid, and contains at least one or more repeating units (A) having a structure in which an alkali soluble group is protected by an acid dissociative dissolution inhibiting group. The so-called acid dissociative dissolution inhibiting group refers to a group that inhibits the dissolution of a polymer in an alkali developer and dissociates and dissolves the polymer in an alkali developer by the action of an acid. In addition, in order to improve the substrate adhesion of the polymer, a repeating unit (B) having a lactone ring structure, a repeating unit (C) having a hydroxyl group, etc. are sometimes included. In addition, as required, other repeating units such as a repeating unit (D) having a structure that inhibits dissolution in an alkali developer and is stable under the action of an acid (hereinafter, sometimes referred to as an "acid stability dissolution inhibiting structure") may be included.

[0041] (Repeating unit (A))

[0042] The repeating unit (A) is a repeating unit having a structure in which an alkali-soluble group such as a carboxyl group, a phenolic hydroxyl group or a sulfonic acid group is protected by an acid-dissociable dissolution-inhibiting group that can dissociate under the action of an acid. Preferably, the repeating unit is a repeating unit in which an OH group such as a carboxyl group, a phenolic hydroxyl group or a sulfonic acid group in a repeating unit derived from (meth)acrylic acid or hydroxystyrene is protected by an acid-dissociable dissolution-inhibiting group.

[0043] Examples of the acid-dissociative dissolution inhibiting group include a structure represented by the formula (a1) or (a2).

[0044] [Chemical formula 1]

[0045]

[0046] In formula (a1), * represents a bonding site in formula (a1), R 20 and R 21 Each independently represents a hydrocarbon group having 1 to 4 carbon atoms, and specific examples thereof include alkyl groups having 1 to 4 carbon atoms such as methyl, ethyl, n-propyl, isopropyl, n-butyl, and isobutyl. 22 represents a hydrocarbon group having 1 to 12 carbon atoms, and specifically, examples thereof include a linear, branched or cyclic alkyl group having 1 to 12 carbon atoms such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, cyclopentyl, cyclohexyl, norbornyl, tricyclo[5.2.1.02,6]decyl, adamantyl, tetracyclo[4.4.0.12,5.17,10]dodecyl, and an aryl group having 6 to 12 carbon atoms such as phenyl and naphthyl. It should be noted that R 22 Can also be used with R 20 or R 21Specifically, they are alicyclic rings having 5 to 12 carbon atoms, such as cyclopentane ring, cyclohexane ring, norbornane ring, tricyclo[5.2.1.02,6]decane ring, adamantane ring, tetracyclo[4.4.0.12,5.17,10]dodecane ring, etc. 22 Medium or R 22 With R 20 or R 21 When a saturated alicyclic ring, specifically a cyclopentane ring, cyclohexane ring, norbornane ring, tricyclo[5.2.1.02,6]decane ring, adamantane ring, tetracyclo[4.4.0.12,5.17,10]dodecane ring, etc., is bonded, the difference in solubility in an alkaline developer before and after photolithography is large, which is preferred for drawing fine patterns.

[0047] [Chemical formula 2]

[0048]

[0049] In formula (a2), * represents the bonding site of formula (a2), R 23 and R 24 Each independently represents a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms, and specific examples thereof include a hydrogen atom, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and an alkyl group having 1 to 4 carbon atoms. 25 represents a hydrocarbon group having 1 to 12 carbon atoms, and specifically includes a linear, branched or cyclic alkyl group having 1 to 12 carbon atoms such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, 2-ethylhexyl, cyclopentyl, cyclohexyl, norbornyl, tricyclo[5.2.1.02,6]decyl, adamantyl, tetracyclo[4.4.0.12,5.17,10]dodecyl. 23 Can also be used with R 24 or R 25 bonded to form a ring, respectively, as R 23 With R 24 Specific examples of the ring formed by bonding include cyclopentane ring, cyclohexane ring, norbornane ring, tricyclo[5.2.1.02,6]decane ring, adamantane ring, tetracyclo[4.4.0.12,5.17,10]dodecane ring, and the like. 23 With R 25 Specific examples of the ring formed by bonding include a hydrogenated furan ring and a hydrogenated pyran ring.

[0050] Specific examples of the repeating unit (A) are given below, but the present invention is not limited thereto. One or more repeating units (A) having different structures can be selected and used.

[0051] [Chemical formula 3]

[0052]

[0053] (Where R x represents H, CH3 or CF3. )

[0054] [Chemical formula 4]

[0055]

[0056] (Where R x represents H, CH3 or CF3. )

[0057] (Repeating unit (B))

[0058] The repeating unit (B) is a repeating unit having a lactone structure or a sultone structure, and imparts the following functions: improving adhesion to a substrate or a base film, or controlling solubility in a photolithography solvent or an alkaline developer. As a preferred example, the structure represented by formula (B1) can be cited.

[0059] [Chemical formula 5]

[0060]

[0061] In formula (B1), R 30 represents a hydrocarbon group having 1 to 4 carbon atoms which may be substituted by a hydrogen atom or a fluorine atom, and specifically includes alkyl groups having 1 to 4 carbon atoms such as a hydrogen atom, a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, and a trifluoromethyl group, preferably a hydrogen atom, a methyl group, and a trifluoromethyl group. 31 represents a single bond or a divalent linking group. The divalent linking group represents an alkylene group having 1 to 4 carbon atoms, or a group in which the alkylene group is substituted with an oxygen atom, a carbonyl group or a carbonyloxy group. 32 It represents a lactone structure-containing group represented by formula (b).

[0062] [Chemical formula 6]

[0063]

[0064] In formula (b), R 301 ~R 308 Any one of the above is represented as R 32 The bonding site is a single bond, and the remaining R 301 ~R 308 represents a hydrogen atom, a hydrocarbon group having 1 to 4 carbon atoms, or an alkoxy group, or R 301 ~R 308 Any one of the above indicates that R 32 bonding site and can bond with other R 301 ~R 308Any one or two of them are bonded to form an alicyclic group having 5 to 15 carbon atoms, a hydrocarbon group having 3 to 14 carbon atoms which may contain an oxygen atom or a sulfur atom, and the remaining R 301 ~R 308 Any one or two of them represent single bonds for forming the alicyclic ring having 5 to 15 carbon atoms, and the other R 301 ~R 308 represents a hydrogen atom, a hydrocarbon group having 1 to 4 carbon atoms, or an alkoxy group. m represents an integer of 0 or 1.

[0065] Specific examples of the above-mentioned alicyclic ring include cyclopentane ring, cyclohexane ring, norbornane ring, 7-oxa-norbornane ring, 7-thia-norbornane ring, tetracyclo[4.4.0.12,5.17,10]dodecane ring, etc., preferably norbornane ring and 7-oxa-norbornane ring. Specific examples of hydrocarbon groups having 1 to 4 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, etc., and specific examples of alkoxy groups having 1 to 4 carbon atoms include methoxy, ethoxy, etc.

[0066] In formula (b), R 301 ~R 308 Any one of the above indicates that R 32 The single bond of the bonding site, the remaining R 301 ~R 308 Particularly preferred examples of the lactone structure representing a hydrogen atom or a hydrocarbon group or alkoxy group having 1 to 4 carbon atoms include a γ-butyrolactone structure and a δ-valerolactone structure. 301 ~R 308 Any one of the above indicates that R 32 bonding site and can bond with other R 301 ~R 308 Any one or two of them are bonded to form an alicyclic group having 5 to 15 carbon atoms, a hydrocarbon group having 3 to 14 carbon atoms which may contain an oxygen atom or a sulfur atom, and the remaining R 301 ~R 308 Particularly preferred examples of the lactone structure representing a hydrogen atom or a hydrocarbon group or alkoxy group having 1 to 4 carbon atoms include a 1,3-cyclohexyl lactone structure, a 2,6-norbornane lactone structure, a 7-oxa-2,6-norbornane lactone structure, and a 4-oxa-tricyclo[5.2.1.02,6]decan-3-one structure.

[0067] Specific examples of the repeating unit (B) are given below, but the present invention is not limited thereto. One or more repeating units (B) having different structures can be selected and used.

[0068] [Chemical formula 7]

[0069]

[0070] (Where R x represents H, CH3 or CF3. )

[0071] (Repeating unit (C))

[0072] The repeating unit (C) is a repeating unit having a hydroxyl group or a carboxyl group in a side chain, and imparts the following functions: improving the adhesion between the polymer and the substrate or base film, controlling the solubility in photolithography solvents and alkaline developers, or reacting with a curing agent to form a crosslinked structure.

[0073] As the structure of the repeating unit (C), structures represented by formulae (C1) to (C3) are particularly preferred.

[0074] [Chemical formula 8]

[0075]

[0076] In formula (C1), R 10 represents a hydrocarbon group having 1 to 4 carbon atoms which may be substituted by a hydrogen atom or a fluorine atom, and specifically includes an alkyl group having 1 to 4 carbon atoms which may be substituted by a fluorine atom, such as a hydrogen atom, a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, and a trifluoromethyl group, preferably a hydrogen atom, a methyl group, and a trifluoromethyl group. 11 is a substituted or unsubstituted aromatic hydrocarbon group. 12 represents a single bond or a divalent hydrocarbon group having 1 to 4 carbon atoms which may be substituted with a fluorine atom, or a carbonyl group. Specifically, examples thereof include a single bond, a methylene group, a 1,1-ethylene group, a 2,2-propylene group, a 1,1,1,3,3,3-hexafluoro-2,2-propylene group, a 1,1,1-trifluoro-2-trifluoromethyl-2,3-propylene group and an alkylene group having 1 to 4 carbon atoms which may be substituted with a fluorine atom, preferably a single bond, a 1,1,1,3,3,3-hexafluoro-2,2-propylene group, a 1,1,1-trifluoro-2-trifluoromethyl-2,3-propylene group, and particularly preferably a single bond. i represents an integer of 1 or 2.

[0077] [Chemical formula 9]

[0078]

[0079] In formula (C2), R 13 represents a hydrocarbon group having 1 to 4 carbon atoms which may be substituted by a hydrogen atom or a fluorine atom, and specifically includes an alkyl group having 1 to 4 carbon atoms which may be substituted by a fluorine atom, such as a hydrogen atom, a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, and a trifluoromethyl group, preferably a hydrogen atom, a methyl group, and a trifluoromethyl group. 14R represents a divalent to tetravalent hydrocarbon group having 2 to 20 carbon atoms which may contain a fluorine atom, an oxygen atom or a sulfur atom. Specifically, examples thereof include a linear or branched saturated hydrocarbon group having 2 to 6 carbon atoms such as an ethylene group and an isopropylene group, an aliphatic cyclic group having 5 to 20 carbon atoms which may contain an oxygen atom or a sulfur atom such as a cyclohexane ring, a norbornane ring, a 7-oxa-norbornane ring, a 7-thia-norbornane ring, an adamantane ring, a tetracyclo[4.4.0.12,5.17,10]dodecane ring, and an aromatic group having 6 to 20 carbon atoms such as a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, and a biphenyl ring. Preferably, the ring is a cyclohexane ring, a norbornane ring, an adamantane ring, or a benzene ring. 15 represents a single bond or a divalent hydrocarbon group having 1 to 4 carbon atoms which may be substituted with a fluorine atom, and specifically includes an alkylene group having 1 to 4 carbon atoms which may be substituted with a fluorine atom, such as a single bond, a methylene group, a 1,1-ethylene group, a 2,2-propylene group, a 1,1,1,3,3,3-hexafluoro-2,2-propylene group, and a 1,1,1-trifluoro-2-trifluoromethyl-2,3-propylene group, and preferably a single bond, a 1,1,1,3,3,3-hexafluoro-2,2-propylene group, and a 1,1,1-trifluoro-2-trifluoromethyl-2,3-propylene group. j represents an integer of 1 to 3.

[0080] [Chemical formula 10]

[0081]

[0082] In formula (C3), R 16 R represents a hydrocarbon group having 1 to 4 carbon atoms which may be substituted by a hydrogen atom or a fluorine atom, and specifically includes an alkyl group having 1 to 4 carbon atoms which may be substituted by a fluorine atom, such as a hydrogen atom, a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, and a trifluoromethyl group, preferably a hydrogen atom, a methyl group, and a trifluoromethyl group. 17 represents a divalent alicyclic hydrocarbon group having 6 to 12 carbon atoms which may contain an oxygen atom or a sulfur atom, and specifically includes an alicyclic hydrocarbon group having a norbornane ring, a 7-oxa-norbornane ring, a 7-thia-norbornane ring, a tetracyclo[4.4.0.12,5.17,10]dodecane ring or the like which may contain an oxygen atom or a sulfur atom, and preferably a norbornane ring or a tetracyclo[4.4.0.12,5.17,10]dodecane ring. k represents an integer of 0 or 1.

[0083] Specific examples of the repeating unit (C) are given below, but the present invention is not limited thereto. One or more repeating units (C) having different structures can be selected and used.

[0084] [Chemical formula 11]

[0085]

[0086] (Where R xrepresents H, CH3 or CF3. )

[0087] (Repeating unit (D))

[0088] The repeating unit (D) is a repeating unit having a structure in which an alkali-soluble group such as a carboxyl group or a phenolic hydroxyl group is protected by an acid-stable dissolution-inhibiting group that does not dissociate even under the action of an acid. Preferably, the repeating unit is a repeating unit in which a carboxyl group or a phenolic hydroxyl group in a repeating unit derived from (meth)acrylic acid or hydroxystyrene is protected by an acid-stable dissolution-inhibiting group. The repeating unit imparts the following functions: control of solubility in a photolithography solvent or an alkaline developer, optical properties such as the refractive index and light transmittance of the film, and the like.

[0089] Examples of the acid-stable dissolution inhibiting group include aliphatic hydrocarbon groups with 1 to 12 carbon atoms, aromatic hydrocarbon groups, or structures to which a methyl group or 1-adamantyl group is bonded, wherein the carbon atom bonded to the oxygen atom is a primary or secondary carbon atom replaced by the hydrogen atom of the carboxyl group or the phenolic hydroxyl group. Specifically, examples include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, cyclopentyl, cyclohexyl, 2-norbornyl, 2-isobornyl, 8-tricyclo[5.2.1.02,6]decyl, 1-adamantyl, 2-adamantyl, 4-tetracyclo[4.4.0.12,5.17,10]dodecyl, phenyl, benzyl, naphthyl, anthracenyl, and the like.

[0090] Specific examples of the repeating unit (D) are given below, but the present invention is not limited thereto. One or more repeating units (D) having different structures can be selected and used.

[0091] [Chemical formula 12]

[0092]

[0093] (Where R x represents H, CH3 or CF3. )

[0094] In addition, examples of repeating units having the same effects as those of the repeating unit (D) include repeating units represented by the formula (D').

[0095] [Chemical formula 13]

[0096]

[0097] In formula (D'), R 60 R represents a hydrocarbon group having 1 to 4 carbon atoms which may be substituted by a hydrogen atom or a fluorine atom, and specifically includes an alkyl group having 1 to 4 carbon atoms which may be substituted by a fluorine atom, such as a hydrogen atom, a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, and a trifluoromethyl group, preferably a hydrogen atom, a methyl group, and a trifluoromethyl group. 61is a hydrogen atom, or 62 Specific examples of the bonded single bond or alkylene group having 1 to 4 carbon atoms include a hydrogen atom, a single bond, a methylene group, an ethylene group, an isopropylene group, and the like. 62 It is an aromatic hydrocarbon group having 6 to 14 carbon atoms, and specific examples thereof include a benzene ring, a naphthalene ring, and an anthracene ring.

[0098] Specific examples of the repeating unit (D') are given below.

[0099] [Chemical formula 14]

[0100]

[0101] (Weight average molecular weight·Molecular weight distribution)

[0102] The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the polymer are not particularly limited and can be appropriately set according to the application. In the case of a resist polymer, the weight average molecular weight (Mw) is, for example, 1,000 to 100,000, and the molecular weight distribution (Mw / Mn) is, for example, 1.1 to 5.0.

[0103] In the present invention, the weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of a polymer are measured values ​​obtained by GPC (gel permeation chromatography), and can be measured under the measurement conditions described below.

[0104] [Method for producing polymer solution]

[0105] The method for producing a polymer solution of the present invention includes a first concentration step, a prepolymer solution preparation step, and a second concentration step. In addition, after the second concentration step, a component adjustment step may also be included. In addition, the method for producing a polymer solution of the present invention may also include a solvent replacement step and / or a filtration step before the first concentration step. In addition, the method for producing a polymer solution may also include a polymerization step before the solvent replacement step, and may also include a purification step after the polymerization step. According to a particularly preferred embodiment of the present invention, the method for producing a polymer solution includes, in sequence, a polymerization step, a purification step, a solvent replacement step, a first concentration step, a prepolymer solution preparation step, and a second concentration step.

[0106] [Polymerization process]

[0107] As the polymerization method of the polymer, known polymerization methods such as solution polymerization, emulsion polymerization, suspension polymerization, bulk polymerization, etc. can be cited. Among them, when producing a polymer for resist, solution polymerization is preferred, and it can be implemented by referring to literature related to various known polymerization methods for resist polymers.

[0108] For example, it includes: a heating method in which the monomer and the polymerization initiator are dissolved in a solvent together, and directly heated to polymerize; a drop polymerization method in which the monomer and the polymerization initiator are dropped into a heated solvent to polymerize. In addition, the drop polymerization method includes: a mixed drop method in which the monomer and the polymerization initiator are dissolved in a solvent as required, and dropped into a heated solvent to polymerize; an independent drop method in which the monomer and the polymerization initiator are dissolved in a solvent as required, and dropped into a heated solvent to polymerize; etc. In the present invention, the drop polymerization method is preferred.

[0109] Here, with regard to the method of heating up together, in the polymerization system, in addition, with regard to the mixed dropping method, in the dropping liquid storage tank before being added dropwise to the polymerization system, there is an opportunity to contact with low-concentration free radicals in a state where the concentration of the monomer is high, therefore, there is a tendency to easily generate a high molecular weight body (polymer) of more than 100,000 molecular weight as one of the causes of pattern defects. On the other hand, with regard to the independent dropping method, in the dropping liquid storage tank, the polymerization initiator and the monomer do not coexist, and the state of low monomer concentration is also maintained when being added dropwise to the polymerization system, thus, it is not easy to generate a polymer, therefore, as the polymerization method in the present invention, the independent dropping method is particularly preferably used. It should be noted that in the mixed dropping method and the independent dropping method, the composition of the monomer added dropwise, the composition ratio of the monomer, the polymerization initiator and the chain transfer agent, etc. can be changed with the dropping time.

[0110] The polymerization initiator can use a known polymerization initiator. As a polymerization initiator for free radical polymerization, for example, a free radical polymerization initiator such as an azo compound or a peroxide is preferred. As a specific example of a polymerization initiator of an azo compound, 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2-methylpropionic acid) dimethyl ester, 1,1'-azobis(cyclohexane-1-carbonitrile), 4,4'-azobis(4-cyanovaleric acid) and the like can be cited. As a specific example of a polymerization initiator of a peroxide, decanoyl peroxide, lauroyl peroxide, benzoyl peroxide, peroxide bis(3,5,5-trimethylhexanoyl), peroxysuccinic acid, peroxy-2-ethylhexanoic acid tert-butyl ester, peroxy-pivalic acid tert-butyl ester, peroxy-2-ethylhexanoic acid 1,1,3,3-tetramethylbutyl ester and the like can be cited. They can be used alone or in combination. Azo compound polymerization initiators are more preferred because of their excellent handling safety. The amount of the polymerization initiator used can be selected according to the target molecular weight, types of monomers, polymerization initiators, chain transfer agents, solvents, repeating unit composition, polymerization temperature, dropping speed, and the like.

[0111] The polymerization initiator is preferably added to the polymerization system in a state dissolved in an organic solvent. The organic solvent in which the polymerization initiator is dissolved is not particularly limited as long as it can dissolve the polymerization initiator. As a specific example, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl isoamyl ketone, methyl amyl ketone, cyclohexanone, alcohols such as methanol, ethanol, isopropanol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, ether alcohols such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ether esters such as methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, methyl propionate, methyl lactate, ethyl lactate, esters such as esters, tetrahydrofuran, 1,4-dioxane, ethylene glycol dimethyl ether, aromatic hydrocarbons such as toluene and xylene, N,N-dimethylformamide, acetonitrile, etc. can be cited. These solvents may be used alone or in combination of two or more.

[0112] The chain transfer agent can use substances known as chain transfer agents as needed. Among them, it is preferably a thiol compound, which can be widely selected from known thiol compounds. Specifically, tert-dodecyl mercaptan, mercaptoethanol, thioglycolic acid, mercaptopropionic acid, etc. can be cited. In addition, the thiol compound having a structure in which 2-hydroxy-1,1,1,3,3,3-hexafluoro-2-propyl is bonded to a saturated aliphatic hydrocarbon has the effect of suppressing the roughness and defects of the photolithographic pattern, and is therefore particularly preferred. The amount of the chain transfer agent used can be selected according to the target molecular weight, monomer, polymerization initiator, chain transfer agent and solvent, etc., repeating unit composition, polymerization temperature, drop rate, etc.

[0113] As for the monomer and polymerization initiator in the dropwise addition liquid, when it is liquid itself, it can also be directly supplied without being dissolved in the solvent, but when the monomer or polymerization initiator is a viscous liquid or solid, it needs to be dissolved in the solvent for use. The higher the concentration of the monomer and polymerization initiator is from the perspective of productivity, the better, but if the concentration is too high, the solution viscosity becomes higher and the operability becomes worse, and when the monomer or polymerization initiator is solid, it precipitates, or it takes time to diffuse in the polymerization system, and sometimes it is easy to generate a high polymer. Therefore, it is preferred that within the viscosity range where there is no problem in the supply operation, each monomer and polymerization initiator can be fully dissolved, and will not precipitate during supply, and the concentration that is easy to diffuse in the polymerization system is selected. The specific concentration varies according to the combination of the solute and the solvent of each solution, and is usually prepared in a manner such that the total concentration of all monomers and the concentration of the polymerization initiator are each 5 to 60% by mass, preferably 10 to 50% by mass.

[0114] When the dropping time in the mixed dropping method and the independent dropping method is short, the molecular weight distribution tends to become broad, and the temperature of the polymer solution decreases due to the dropping of a large amount of solution at a time, so it is not preferred. On the contrary, when the dropping time is long, the polymer is given a thermal history that is more than necessary, and the productivity decreases, so it is not preferred. Therefore, it is usually selected from the range of 0.5 to 24 hours, preferably 1 to 12 hours, and particularly preferably 2 to 8 hours.

[0115] In addition, after the addition is completed and the temperature is raised to the polymerization temperature in the simultaneous temperature raising method, it is preferred to maintain the temperature for a certain period of time, or further raise the temperature to ripen the remaining unreacted monomers. If the ripening time is too long, the production efficiency per unit time is reduced, and the polymer is given a thermal history that is more than necessary, so it is not preferred. Therefore, it is usually selected from within 12 hours, preferably within 6 hours, and particularly preferably within 1 to 4 hours.

[0116] The solvent used in the polymerization reaction is not particularly limited as long as it is a solvent that can stably dissolve the raw material monomers, the obtained polymer, the polymerization initiator and the chain transfer agent. Specific examples of the polymerization solvent include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl isoamyl ketone, methyl amyl ketone, and cyclohexanone, alcohols such as methanol, ethanol, and isopropanol, ether alcohols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether, esters such as methyl acetate, ethyl acetate, isopropyl acetate, propyl acetate, butyl acetate, methyl propionate, methyl lactate, and ethyl lactate, ether esters such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate, tetrahydrofuran, 1,4-dioxane, and ethylene glycol dimethyl ether, aromatic hydrocarbons such as toluene and xylene, N,N-dimethylformamide, and acetonitrile. Considering the solubility and boiling point of monomers, polymerization initiators, chain transfer agents, and polymers, acetone, methyl ethyl ketone, methyl isobutyl ketone, isopropanol, propylene glycol monomethyl ether, methyl acetate, ethyl acetate, isopropyl acetate, propyl acetate, methyl propionate, tetrahydrofuran, 1,4-dioxane, ethylene glycol dimethyl ether, toluene, and acetonitrile are preferred. They can be used alone or in combination of two or more. In addition, ethylene glycol monobutyl ether, 3-methoxy-3-methyl-1-butanol, 3-methoxy-3-methyl-1-butyl acetate, 3-ethoxypropionic acid ethyl ester, γ-butyrolactone, diethylene glycol dimethyl ether, N-methylpyrrolidone, dimethyl sulfoxide, and other compounds with high solubility and high boiling point for monomers, polymerization initiators, chain transfer agents, and polymers can also be used in combination.

[0117] The amount of the polymerization solvent is not particularly limited, but if the amount of the solvent is too little, the monomer may be precipitated or the viscosity may be too high to keep the polymerization system uniform, and if the amount of the solvent is too much, the conversion rate of the monomer may be insufficient or the molecular weight of the polymer may not be increased to a desired value. Usually, the amount is 0.5 to 20 parts by mass, preferably 1 to 10 parts by mass, relative to 1 part by mass of the monomer.

[0118] The amount of polymerization solvent (hereinafter sometimes referred to as initial charge solvent) initially charged into the reaction tank in the mixed dropwise method and the independent dropwise method may be at least the minimum amount for stirring. If it is more than the necessary amount, the amount of monomer solution that can be supplied becomes less, and the production efficiency is reduced, which is not preferred. Usually, relative to the final input amount (i.e., the total amount of the initial charge solvent, the monomer solution and the initiator solution added dropwise), it is selected from a range of, for example, 1 / 30 or more, preferably 1 / 20 to 1 / 2, and particularly preferably 1 / 10 to 1 / 3 in terms of volume ratio. It should be noted that a part of the monomers may also be mixed in the initial charge solvent in advance.

[0119] The polymerization temperature can be appropriately selected according to the boiling points of the solvent, monomer, chain transfer agent, etc., the half-life temperature of the polymerization initiator, etc. At low temperatures, it is difficult to polymerize, so there are problems in terms of productivity. In addition, if it is set to a high temperature higher than necessary, there are problems in terms of the stability of the monomer and the polymer. Therefore, it is preferably selected in the range of 40 to 160°C, particularly preferably 60 to 120°C. The polymerization temperature greatly affects the molecular weight and copolymer composition of the polymer, so it must be precisely controlled. On the other hand, the polymerization reaction is usually an exothermic reaction, and there is a tendency for the polymerization temperature to rise, so it is difficult to control it to a constant temperature. Therefore, in the present invention, it is preferred that, as a polymerization solvent, at least one or more compounds having a boiling point close to the target polymerization temperature are contained, and the polymerization temperature is set to be above the initial boiling point of the compound under the polymerization pressure. According to this method, the rise in the polymerization temperature can be suppressed by utilizing the latent heat of vaporization of the polymerization solvent.

[0120] The polymerization pressure is not particularly limited and may be any pressure under normal pressure, pressure or reduced pressure, but is usually normal pressure. Preferably, in the case of free radical polymerization, when the initiator generates free radicals, the polymerization system is made an open system and carried out near atmospheric pressure; in the case of an azo system, since nitrogen is generated, the polymerization system is made an open system and carried out near atmospheric pressure to suppress the change of polymerization pressure; in the case of a peroxide system, since oxygen is generated, the polymerization system is made an open system and carried out near atmospheric pressure to suppress the change of polymerization pressure.

[0121] [Purification process]

[0122] The polymer after the polymerization reaction contains low molecular weight impurities such as polymerization solvent, unreacted monomers, oligomers, polymerization initiators, chain transfer agents and their reaction byproducts, which are preferably removed by a purification process. Specifically, it can be carried out in the following ways: precipitation purification, that is, the polymerization reaction solution is diluted by adding a good solvent as needed, and then it is contacted with a poor solvent to precipitate the polymer and extract the impurities into the poor solvent phase; or, it is made into a liquid-liquid two-phase, and the impurities are extracted into the poor solvent phase. The polymer separated by precipitation purification can also be further washed with a poor solvent. These operations can be repeated in the same way, or different operations can be combined.

[0123] As the poor solvent used in this purification process, compounds with hydroxyl groups such as water, methanol, ethanol, isopropanol, ethylene glycol, ethyl lactate, pentane, normal hexane, isohexane, normal heptane, cyclopentane, methylcyclohexane, straight-chain, branched or cyclic saturated hydrocarbons or aromatic hydrocarbons such as toluene and dimethylbenzene can be enumerated. These solvents can be used alone or mixed with more than two kinds. In addition, as good solvent, solvents exemplified in the above-mentioned polymerization solvent, the film forming solvent described later, etc. can be enumerated, and poor solvents can also be mixed in good solvents and used.

[0124] The type and amount of the poor solvent used in the purification process are not particularly limited as long as they can separate the polymer from the low molecular weight compound, and can be appropriately selected according to the solubility of the polymer in the poor solvent, the type and amount of the solvent used in the polymerization, the type and amount of impurities, etc. When the amount of the poor solvent is small, the separation of impurities such as the polymerization solvent and the unreacted monomer becomes insufficient. On the contrary, when the amount of the poor solvent is too much, the waste liquid increases, etc., which is not preferred from the perspective of workability and cost. Usually, the mass ratio is 0.5 to 50 times, preferably 1 to 20 times, and more preferably 2 to 10 times, relative to the total mass of the polymerization reaction solution diluted with a good solvent as needed.

[0125] The temperature of the purification process greatly affects the molecular weight, molecular weight distribution, removal rate of impurities such as residual monomers and initiator residues, and various characteristics in photolithography of the polymer, so it must be strictly controlled. When the temperature of the purification process is too low, the solubility of impurities in the reprecipitation solvent and the washing solvent becomes insufficient, and the impurities cannot be fully removed, so it is not efficient. On the contrary, when the temperature of the purification process is too high, the polymer is eluted into the reprecipitation solvent and the washing solvent, and the composition balance in the low molecular weight region of the polymer collapses, or the yield is reduced, so it is not preferred. Therefore, it is preferred that the purification process is carried out at a temperature in the range of 0 to 40°C, preferably in the range of 0 to 30°C.

[0126] A treatment for removing metal impurities contained in the polymer may also be performed. As for the method, a solution obtained by dissolving the polymer in an organic solvent may be washed with pure water, or the solution may be brought into contact with an ion exchange resin, or the solution may be passed through a filter having an ion exchange capacity. In addition, these methods may be combined. Ion exchange resins and filters having an ion exchange capacity may use known commercial products used for metal removal of resist polymers.

[0127] [Solvent replacement process]

[0128] The solvent replacement step is a step of replacing the solvent of the polymer solution with a solvent used for the resist composition or the like.

[0129] The replacement method is implemented by heating the polymer solution under reduced pressure, distilling off low-boiling substances such as the solvent used in purification, supplying the resist solvent thereto, and further distilling off the initial solvent together with the supplied solvent. Low-boiling impurities such as the solvent used in purification can be removed, and the polymer can be refined into a resist solution.

[0130] The temperature of the heat source during reduced pressure heating is not particularly limited as long as it is a temperature at which the polymer does not denature, but is usually preferably 100°C or less, more preferably 70°C or less, further preferably 60°C or less, and particularly preferably 50°C or less. In the solvent replacement process, the low boiling point component and the finishing solvent are evaporated under reduced pressure, so the polymer solution in the process is cooled by the heat of vaporization, and its temperature becomes lower than the temperature of the heat source. By limiting the temperature of the heat source, it is possible to prevent the polymer from being deteriorated due to overheating.

[0131] In addition, when replacing the solvent, if the amount of the solvent supplied subsequently is too small, the low boiling point compounds cannot be fully removed, and if it is too large, the replacement takes time and the polymer is given a thermal history that is more than necessary, which is not preferred. The supply amount can usually be selected from the range of 1.05 to 10 times, preferably 1.1 to 5 times, and particularly preferably 1.2 to 3 times the amount required as the solvent of the finishing solution.

[0132] As the displacement solvent, there is no particular limitation as long as the polymer can be dissolved. For example, if the displacement solvent is for resist purposes, known resist solvents commonly used in resist compositions can be used. Specifically, solvents such as propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol n-butyl ether, dipropylene glycol n-propyl ether, dipropylene glycol n-butyl ether, ethyl lactate, methyl amyl ketone, γ-butyrolactone, cyclohexanone, and 4-methyl-2-pentanol can be cited.

[0133] Solvent substitution can be substituted with a single solvent or a mixed solvent using more than two solvents. When substituted with a single solvent, which solvent to use among the multiple solvents used for the target polymer solution is selected by considering the polymer solubility of each solvent, the boiling point difference, the solvent composition ratio of the target polymer solution, etc.

[0134] For example, from the perspective of polymer solubility, any of a variety of solvents used for the target polymer solution may be used as long as the polymer solubility can be maintained in the subsequent first concentration step, but it is preferably replaced with a solvent with a higher polymer solubility because the polymer solution can be concentrated to a high concentration in the first concentration step without worrying about polymer precipitation.

[0135] On the other hand, when the boiling point difference of each solvent is large and the composition of the high boiling point solvent in the target solvent composition is not so large, if it is replaced with a high boiling point solvent, the subsequent process may not be continued. For example, in the case of manufacturing with the target of 50% by mass of polymer concentration and X / Y composition ratio of mixed solvent = 67 / 33 (boiling point: X<<Y), the composition of the polymer liquid is 100 parts of polymer, 67 parts of solvent X, and 33 parts of solvent Y. If the solvent Y is not concentrated to less than 33 parts in the first concentration step after the solvent replacement, it is predicted that it will be difficult to distill and remove the solvent Y in the second concentration step after the solvent X is supplemented, so there is a concern that the target composition of X:Y cannot be achieved. However, when the solvent Y is concentrated to 33 parts by mass relative to 100 parts of the polymer in the first concentration step, the possibility of a large amount of polymer precipitation is high, which is not realistic. In such a case, it is advisable to replace it with a low boiling point solvent X in the solvent replacement step.

[0136] [Filtration process]

[0137] In addition, in order to remove the microgel of the polymer which is not preferred due to the pattern defect of the resist, it is preferred to filter the polymer solution using a filter. The filtration accuracy of the filter is less than 0.2 μm, preferably less than 0.1 μm, and particularly preferably less than 0.05 μm. The material of the filter can include polyolefins such as polyethylene and polypropylene, resins containing polar groups such as polyamide, polyester, polyacrylonitrile, and fluorinated polyethylene. Fluorine-containing resins, particularly preferably polyamide. As examples of polyamide-based filters, (hereinafter referred to as trademarks) Ultipleat P-nylon 66, Ultipor N66 made by Pall (Strain) of Japan, LifeASSURE PSN series, LifeASSURE EF series made by CUNO (Strain), etc. can be cited. As polyolefin-based filters, Microgard Plus HC10, Optimizer D, etc. made by Nihon Entegris KK can be cited. These filters can be used alone or in combination of two or more.

[0138] The filtration step may be performed after the purification step, after the solvent replacement step, or after both steps.

[0139] [Preparation of polymer solutions containing various solvents]

[0140] The polymer solution produced by the method of the present invention contains C mass % of a polymer in a mixed solvent obtained by mixing at least two or more solvents at a predetermined mass ratio.

[0141] The type of solvent is not limited as long as it can dissolve the polymer uniformly. For example, in a mixed solvent, a solvent of the same type as the above-mentioned replacement solvent can be used. In the case of a resist polymer solution, it is preferred to contain a resist solvent of the same type as the solvent used in the resist composition.

[0142] The mass ratio of each solvent is not limited as long as the polymer can be uniformly dissolved. In the present invention, when n kinds of solvents are included in the mixed solvent, each solvent is set as the first solvent, ..., the nth solvent, and the concentration of each solvent is set as the first solvent ≥ ... ≥ the nth solvent. For example, when two kinds of solvents are included in the mixed solvent, the concentration of the first solvent is preferably 45% by mass or more and less than 80% by mass, more preferably 50% by mass or more and 75% by mass or less, relative to the total mass of the mixed solvent, and the concentration of the second solvent is preferably 20% by mass or more and 50% by mass or less, more preferably 25% by mass or more and 50% by mass or less. In addition, when three kinds of solvents are included in the mixed solvent, the concentration of the third solvent is preferably greater than 0% by mass and less than 20% by mass, more preferably 1% by mass or more and 15% by mass or less, relative to the total mass of the mixed solvent.

[0143] The polymer concentration C is not limited as long as the polymer can be uniformly dissolved. When the polymer solution is a resist polymer solution, the polymer concentration C is preferably 20 to 70% by mass, and particularly in the case of a thick film resist polymer solution, the polymer concentration C is more preferably 30 to 70% by mass, and further preferably 35 to 65% by mass.

[0144] The present invention is a method for producing a polymer solution containing C mass % of a polymer in a mixed solvent obtained by mixing at least two or more solvents in a specified mass ratio, wherein the polymer concentration and solvent composition of a "prepolymer solution" such that the solvent composition will just be the desired value when the polymer solution containing all of the aforementioned solvents is concentrated to a target concentration of C mass % is estimated, and after the prepolymer solution is prepared, it is concentrated to thereby produce the target polymer solution.

[0145] [Preparation of prepolymer solution]

[0146] The so-called prepolymer solution in the present invention refers to the following polymer solution: it is a polymer solution having a lower polymer concentration than the polymer solution containing at least two or more solvents to be produced by the present invention, and contains the same type of solvents, and when concentrated to a target polymer concentration, the solvent composition ratio becomes the target composition ratio.

[0147] The polymer concentration Ck% by mass of the prepolymer solution must be lower than the polymer concentration C% by mass of the target polymer solution, but if it is too low, the amount of solvent discarded by concentration increases, which is not preferred. The preferred range of Ck is 0.3C to 0.8C, and more preferably 0.4C to 0.7C.

[0148] The solvent composition of the prepolymer solution must be set so that the desired composition ratio is obtained when the prepolymer solution is concentrated from the polymer concentration Ck to the target concentration C. Since the boiling point and vapor pressure vary depending on the type of solvent, it is necessary to estimate the extent to which each of the mixed solvents is removed by distillation when performing concentration by distillation. The volatility data of the solvent used in the design of the distillation can be obtained in various ways, for example, simulation can also be performed based on the correlation diagram of the gas phase composition / liquid phase composition of the gas-liquid equilibrium.

[0149] In addition, as a simple method, it is also possible to imagine concentrating a prepolymer solution with a polymer concentration of Ck mass % to a polymer concentration of C mass %, finding the proportion of the solvent remaining at the bottom by calculation, temporarily setting the solvent composition ratio before concentration with reference to the boiling point and vapor pressure of each solvent, and trying to concentrate the mixed solvent with the temporarily set composition ratio to the ratio found by the above calculation, and confirming how the solvent composition ratio changes.

[0150] Specifically, the mass ratio of each solvent in the prepolymer solution can be determined by the following preliminary test.

[0151] (Preliminary test steps)

[0152] The solvent concentration R when the prepolymer solution having a polymer concentration of Ck mass % is concentrated to a polymer concentration of C mass % can be calculated by the following calculation formula.

[0153] R = (100-C) / (100×C / Ck-C)

[0154] Next, a mixed solvent is prepared in which the composition of the solvent that is expected to be largely removed by distillation based on the boiling point and vapor pressure of each solvent is greater than the target composition, and distillation is performed until the total mass of the mixed solvent is reduced to a value obtained by multiplying the value by the concentration R, and the solvent composition ratio after distillation is obtained. The mixed solvent composition ratio is obtained so that the solvent composition ratio after distillation becomes equal to the target composition, and this mixed solvent composition ratio is used as the mass ratio of each solvent in the prepolymer solution.

[0155] For example, when a prepolymer solution containing two solvents (H and L) with different boiling points and having a polymer concentration of 30% is concentrated, and it is assumed that a polymer solution with a polymer concentration of 50% and H:L=50:50 (mass ratio) is produced, the above-mentioned concentration R is 0.43, which means that if the solvent is removed and concentrated until 70 parts by mass of the solvent contained in 100 parts by mass of the solution with a polymer concentration of 30% becomes 70×0.43≈30 parts by mass, then the polymer concentration becomes 50%.

[0156] The solvent L with a lower boiling point will be removed more by distillation. Therefore, considering the boiling point difference between solvents H and L, a mixed solvent with an H:L mass ratio of 45:55, 40:60, etc. is prepared, and a solvent composition ratio is found such that when the distillation is carried out until the mass of the mixed solvent is reduced to 43%, the H:L mass ratio is close to 50:50, and this is set as the solvent composition ratio of the prepolymer solution.

[0157] [First concentration process]

[0158] The first concentration process is the following process: Before preparing the prepolymer solution, a solution obtained by dissolving a polymer in at least one of the solvents (=the same kind of mixed solvent as the target polymer solution) contained in the prepolymer solution is concentrated so that the polymer concentration becomes Cz (0.8C < Cz ≤ C + 10) mass%.

[0159] The polymer solution supplied to the first concentration process can be prepared by dissolving polymer powder in a solvent, or can be a polymer solution obtained by a polymerization reaction of a polymer. From the aspect of omitting the drying process for making polymer powder and the process of redissolving the polymer powder in a solvent, and further being able to prevent the denaturation of the polymer caused by the heat history in the drying process, it is preferable to use a polymer solution obtained by a polymerization reaction. The polymer solution obtained by a polymerization reaction is preferably supplied to the first concentration process after removing impurities such as unreacted monomers, by-products from polymerization initiators, solvents for polymerization and purification, etc. through the aforementioned purification process, solvent replacement process, filtration process, etc., and replacing the solvent with the desired solvent. It should be noted that it is also possible to directly continue vacuum distillation from the solvent replacement process as the first concentration process.

[0160] [Prepolymer solution preparation process]

[0161] In the prepolymer solution preparation process, a necessary amount of a necessary solvent is added to the polymer solution obtained in the first concentration process to prepare a prepolymer solution having the polymer concentration Ck and the solvent composition ratio set by the aforementioned method.

[0162] [Second concentration process]

[0163] In the second concentration process, the prepolymer solution is concentrated by vacuum distillation until the polymer concentration becomes C mass%. In order to prevent the viscosity of the polymer solution from becoming too high due to concentration and becoming impossible to stir, or the polymer from precipitating, heating can also be carried out, but in the case of a polymer for a resist, attention must also be paid to the modification of the polymer caused by heating. The temperature during distillation is preferably 70°C or lower, more preferably 60°C or lower, and further preferably 50°C or lower. In addition, the degree of vacuum during distillation is preferably 20 kPa or lower, more preferably 10 kPa or lower, and further preferably 5 kPa or lower.

[0164] The end point of the second concentration step can be determined based on the polymer concentration of the prepolymer solution, the mass of the solvent removed by distillation through calculation, or the mass of the entire polymer solution.

[0165] The solvent composition (mass ratio) of the polymer solution after the second concentration step is preferably within ±5% of the target composition ratio.

[0166] [Composition adjustment process]

[0167] When the polymer concentration C and the solvent composition ratio slightly deviate from the target values ​​in the second concentration step, they can be adjusted to the target values ​​by further concentrating and / or adding an appropriate amount of necessary solvent and stirring to homogenize the polymer solution.

[0168] Example

[0169] Hereinafter, the present invention will be described in more detail using Examples, but the present invention is not limited to these Examples.

[0170] Table 1 summarizes the target properties of the polymer solutions produced in Examples and Comparative Examples.

[0171] [Table 1]

[0172]

[0173] The abbreviations in Table 1 are as follows.

[0174] ※1

[0175] PHS: 4-Hydroxystyrene

[0176] TBA: tert-butyl acrylate

[0177] Oa: 3-Hydroxy-1-adamantyl acrylate

[0178] PQMA: 4-Hydroxyphenyl Methacrylate

[0179] ※2

[0180] PGMEA: Propylene glycol monomethyl ether acetate

[0181] PGME: Propylene glycol monomethyl ether

[0182] BuOAc: butyl acetate

[0183] DMAc: dimethylacetamide

[0184] [Solvent composition ratio of polymer solution]

[0185] The solvent composition of the mixed solvent was analyzed by gas chromatography.

[0186] Device: GC-2010plus manufactured by Shimadzu Corporation

[0187] Carrier gas: N2

[0188] Detector: FID

[0189] Column: Aglent J&W DB-5 (15m)

[0190] [Quantification of low molecular weight components in polymers]

[0191] The low molecular weight components contained in the polymer solution were quantitatively analyzed by liquid chromatography.

[0192] Measuring device: HLC-8320GPC manufactured by TOSOH

[0193] Detector: Differential Refractive Index (RI) detector

[0194] Column: TOSOH TSKgel superHZ1000×4

[0195] Eluent: Tetrahydrofuran

[0196] Flow rate: 0.35mL / min

[0197] Temperature: 40℃

[0198] [Water content in polymer solution]

[0199] The water content in the polymer solution was analyzed by the Karl Fischer method.

[0200] Device: Hiranuma Sangyo Karl Fischer Coulometric Moisture Meter AQ-2200

[0201] Electrolyte-generator: Sigma-Aldrich HYDRANAL Coulomat AK

[0202] Electrolyte-counter electrode solution: Sigma-Aldrich HYDRANAL Coulomat CG-K

[0203] [Polymer concentration]

[0204] The polymer concentration in the polymer solution was quantified by the following procedure.

[0205] A portion of the polymer solution was collected and measured, and the solution was dried under reduced pressure at 100°C together with the measuring container, and the mass of the remaining dry polymer was measured. The dry polymer was redissolved in tetrahydrofuran, and the amount of solvent remaining in the dry polymer was quantified by GC analysis. The amount of solvent remaining in the dry polymer was subtracted from the mass of the dry polymer, and the resultant value was divided by the collected mass and used as the polymer concentration.

[0206] [Weight average molecular weight and molecular weight distribution of polymer]

[0207] The weight average molecular weight and molecular weight distribution of the polymer synthesized below were measured by GPC (gel permeation chromatography) using polystyrene as a standard. The sample used for analysis was a sample prepared in a tetrahydrofuran solution having a polymer solid content concentration of 2% by mass. The sample injection volume into the device was 50 μL.

[0208] Measuring device: HLC-8220GPC manufactured by TOSOH

[0209] Detector: Differential Refractive Index (RI) detector

[0210] Column: Shodex GPC KF804 × 3 (Showa Denko)

[0211] Eluent: Tetrahydrofuran

[0212] Flow rate: 1.0mL / min

[0213] Temperature: 40℃

[0214] Calibration curve: Prepared using polystyrene standard samples (manufactured by TOSOH)

[0215] [Monomer composition ratio of polymer]

[0216] The monomer composition ratio of the polymer synthesized below is 13 C-NMR analysis.

[0217] Device: Bruker Ascend400

[0218] Deuterated solvent: acetone-d6

[0219] Relaxation reagent: Chromium(III) acetylacetonate

[0220] Measurement temperature: 30℃

[0221] [Metal Analysis of Polymers]

[0222] The metal content of the polymer synthesized below was analyzed by high-frequency inductively coupled plasma mass spectrometry (ICP-MS). The metals determined were 26 elements, including Na, K, Mg, Al, Ca, Cr, Mn, Fe, Ni, Cu, Zn, Pb, Sn, Co, Li, Ti, Ag, W, V, Ba, Pt, Au, As, Cd, Mo and Zr. The analysis value is based on the mass of the solid component of the polymer.

[0223] Apparatus: ICP mass spectrometer (manufactured by Agilent Technologies Inc., trade name: Agilent7500cs)

[0224] Sample preparation: Dilute the polymer solution with N-methyl-2-pyrrolidone

[0225] [Example 1]

[0226] (Polymerization process)

[0227] A p-hydroxystyrene composition obtained by dehydrogenating p-ethylphenol (25% by mass of p-hydroxystyrene, 41% by mass of p-ethylphenol, 23% by mass of methanol, and 11% of water) and tert-butyl acrylate were dissolved in methanol so that the molar ratio of the monomers became 65:35, and AIBN was added as a polymerization initiator to prepare a monomer solution.

[0228] A quarter of the monomer solution was placed in a reaction vessel equipped with a stirrer, a condenser, and a thermometer, and the mixture was heated to 80° C. while being stirred. The remaining three quarters of the monomer solution was added dropwise at a constant rate over 3 hours, and the polymerization reaction was further continued for 1 hour, followed by cooling to room temperature.

[0229] (Purification process)

[0230] The polymer solution was purified by precipitation using toluene as a poor solvent and acetone as a good solvent by a known method to remove impurities such as the polymerization solvent and unreacted monomers contained in the polymer. Then, the polymer was redissolved in ethyl acetate, washed with a 1% by mass oxalic acid aqueous solution, and then repeatedly washed with pure water to remove metal impurities. The metal content contained in the polymer after washing was analyzed, and the results showed that Na and Zn were 2 ppm each, K, Cr, Fe and Sn were 1 ppb each, and other metal elements were less than 1 ppb.

[0231] To the ethyl acetate solution of the polymer after water washing, PGMEA was added while distilling off ethyl acetate at a heat source temperature of 45°C under reduced pressure, ultimately obtaining a PGMEA solution having a polymer concentration of 30% by mass and containing low-boiling-point solvents such as the polymerization solvent and the purification solvent and water contents of less than 0.1% each.

[0232] The properties of the obtained polymer were: PHS:TBA=65:35, weight average molecular weight (Mw)=23,000, and molecular weight distribution (Mw / Mn)=2.5.

[0233] <Determination of Concentration Ck of Prepolymer Solution and Mass Ratio of PGMEA·PGME>

[0234] The polymer concentration Ck of the prepolymer solution was set to 28% by mass. When the prepolymer solution was concentrated to 50% by mass in the second concentration step, the concentration of the solvent R = (100-C) / (100×C / Ck-C) = about 0.4.

[0235] According to the boiling point of PGMEA of 146°C and the vapor pressure of 0.5 kPa (20°C), and the boiling point of PGME of 120°C and the vapor pressure of 1.2 kPa (20°C), it is believed that PGME will be distilled away more during distillation. Therefore, a mixed solvent with a PGME composition greater than 50% of the target was prepared, and a preliminary test was conducted to investigate the solvent composition ratio when the total mass was reduced to 40% under the conditions of reduced pressure of 1 kPa and temperature of 45°C. As a result, if the mixed solvent with a PGMEA / PGME mass ratio of 40:60 is distilled to a concentration of 40%, the PGMEA / PGME mass ratio becomes 52:48, and a value close to the target solvent composition is obtained. From this result, it is predicted that if the prepolymer solution is adjusted in a manner such that the polymer concentration is 28% by mass and the mass ratio of PGMEA / PGME is 40 / 60, when the prepolymer solution is concentrated to a polymer concentration of 50% by mass, a polymer solution close to the target polymer concentration and solvent composition can be obtained.

[0236] (First Concentration Step)

[0237] 400 g of the PGMEA solution having a polymer concentration of 30% by mass obtained in the solvent replacement step was slowly concentrated using an evaporator at a heat source temperature of 45° C. and a reduced pressure of 1 kPa to obtain 240 g of a PGMEA solution having a polymer concentration of 50% by mass. Slight precipitation of the polymer was observed at this time.

[0238] (Prepolymer solution preparation step)

[0239] 180 g of PGME was added to the above solution to dilute it, thereby preparing 420 g of a prepolymer solution having a polymer concentration of 28.6% by mass and a PGMEA:PGME mass ratio of 40:60.

[0240] (Second Concentration Step)

[0241] The prepolymer solution was added to the flask and slowly concentrated under reduced pressure using an evaporator at a reduced pressure of 6 to 10 kPa and a heat source temperature of 45°C. The concentration was completed when the mass of the contents of the flask reached 240 g. The obtained polymer solution was analyzed, and the polymer concentration was 50% by mass, and the solvent composition was PGMEA:PGME=51:49.

[0242] [Example 2]

[0243] (Polymerization process)

[0244] The same polymer solution as in Example 1 was produced on a scale about 8.3 times that of Example 1 (polymer solid content: 1.0 kg).

[0245] The polymerization, purification and solvent replacement were carried out according to Example 1 to prepare a PGME solution of a PHS / TBA copolymer having a polymer concentration of 30% by mass and a low boiling point solvent and water content of less than 0.1% each.

[0246] The concentration Ck and the solvent composition ratio of the prepolymer solution were set to the same values ​​as those in Example 1 (Ck=28% by mass, PGMEA / PGME mass ratio=40 / 60).

[0247] (First Concentration Step)

[0248] 3.33 kg of a PGMEA solution having a polymer concentration of 30% by mass obtained by solvent replacement was slowly concentrated using an evaporator at a heat source temperature of 45° C. and a reduced pressure of 1 kPa until the mass of the polymer solution became 2.0 kg.

[0249] (Prepolymer solution preparation step)

[0250] Then, 1.5 kg of PGME was added for dilution to prepare 3.5 kg of a prepolymer solution.

[0251] (Second Concentration Step)

[0252] The prepolymer solution was slowly concentrated using an evaporator at a heat source temperature of 45°C and a reduced pressure of 6 to 10 kPa until the mass of the polymer solution reached 2.0 kg. A portion of the obtained polymer solution was collected for analysis, and the result showed that the polymer concentration was 51.4% by mass and the solvent composition (mass ratio) was PGMEA:PGME=52.0:48.0.

[0253] (Composition adjustment process)

[0254] Since the polymer concentration was slightly higher than the target value, a small amount of PGME was added to adjust the polymer concentration to 50.1 mass % and the solvent composition (mass ratio) to PGMEA:PGME=50.4:49.6, which was closer to the target composition.

[0255] [Example 3]

[0256] (Polymerization process)

[0257] The same p-hydroxystyrene composition as that used in Example 1 and 3-hydroxy-1-adamantyl acrylate were dissolved in isopropyl alcohol at a monomer molar ratio of 70:30, and dimethyl 2,2-azobisisobutyrate was added as a polymerization initiator to prepare a monomer solution.

[0258] A quarter of the monomer solution was placed in a reaction vessel equipped with a stirrer, a condenser, and a thermometer, and the mixture was heated to 80° C. while being stirred. The remaining three quarters of the monomer solution was added dropwise at a constant rate over 3 hours, and the polymerization reaction was further continued for 1 hour, followed by cooling to room temperature.

[0259] (Purification process)

[0260] The polymerization solution was purified by precipitation using toluene as a poor solvent and an isopropanol / methanol mixed solvent as a good solvent to remove impurities such as the polymerization solvent and unreacted monomers contained in the polymer. The polymer was then redissolved in methanol and passed through a metal removal filter (40QSH manufactured by Sumitomo 3M) with an adsorption effect based on zeta potential and a nylon membrane filter (LifeASSURE manufactured by Sumitomo 3M) with a nominal pore size of 0.04 μm to remove metal impurities and minute insoluble components.

[0261] (Solvent replacement process)

[0262] To the polymer solution after the filter treatment, PGME was added while distilling off methanol at a heat source temperature of 45°C under reduced pressure, to finally obtain a PGME solution having a polymer concentration of 30% by mass and containing low boiling point solvents such as polymerization solvent and purification solvent and water contents of less than 0.1% each.

[0263] The obtained polymer had PHS:Oa=69:31, weight average molecular weight (Mw)=12,000, and molecular weight distribution (Mw / Mn)=1.6.

[0264] <Determination of Concentration Ck of Prepolymer Solution and Mass Ratio of PGMEA·PGME>

[0265] The polymer concentration Ck of the prepolymer solution is set to 23% by mass. When the prepolymer solution is concentrated to 40% by mass in the second concentration step, the concentration of the solvent R=(100-C) / (100×C / Ck-C)=about 0.45.

[0266] A PGMEA / PGME mixed solvent having a PGME composition greater than 50% of the target was prepared in the same manner as in Example 1, and a preliminary test was conducted to investigate the solvent composition ratio when the total mass was reduced to 45% by distillation under the conditions of reduced pressure of 1 kPa and temperature of 45°C. As a result, if a mixed solvent having a PGMEA / PGME mass ratio of 38 / 62 was distilled to a concentration of 45%, the PGMEA / PGME mass ratio became 50 / 50, which is the same value as the target solvent composition. From this result, it is predicted that if the prepolymer solution is adjusted in such a way that the polymer concentration is 23% by mass and the PGMEA / PGME mass ratio is 38 / 62, then when the prepolymer solution is concentrated to a polymer concentration of 40% by mass, a polymer solution having the target polymer concentration and solvent composition can be obtained.

[0267] (First Concentration Step)

[0268] 200 g of the PGME solution having a polymer concentration of 30% by mass obtained in the solvent replacement step was slowly distilled under the conditions of a heat source temperature of 45° C. and a reduced pressure of 10 kPa to obtain 167 g of a PGME solution having a polymer concentration of 36% by mass.

[0269] (Prepolymer solution preparation step)

[0270] To the above solution, 76.3 g of PGMEA and 17.5 g of PGME were added to dilute the solution, thereby preparing 261 g of a prepolymer solution having a polymer concentration of 23% by mass and a PGMEA:PGME mass ratio of 38:62.

[0271] (Second Concentration Step)

[0272] The prepolymer solution was added to the flask and slowly concentrated under reduced pressure using an evaporator at a reduced pressure of 10 kPa and a heat source temperature of 45°C. The concentration was completed when the mass of the contents of the flask reached 150 g. The obtained polymer solution was analyzed, and the polymer concentration was 40% by mass, and the solvent composition was PGMEA:PGME=50.6:49.4.

[0273] [Example 4]

[0274] (Polymerization process)

[0275] The same polymer solution as in Example 3 was produced on a scale about 100 times that of Example 3 (polymer solid content: 6.0 kg).

[0276] The polymerization, purification and solvent replacement were carried out according to Example 1 to prepare a PGME solution of a PHS / Oa copolymer having a polymer concentration of 30% by mass and a low boiling point solvent and water content of less than 0.1% each.

[0277] The concentration Ck and the solvent composition ratio of the prepolymer solution were set to the same values ​​as those in Example 2 (Ck=23% by mass, PGMEA / PGME mass ratio=38 / 62).

[0278] (First Concentration Step)

[0279] 20.0 kg of a PGMEA solution having a polymer concentration of 30% by mass obtained by solvent replacement was slowly concentrated using an evaporator at a heat source temperature of 45°C and a reduced pressure of 1 kPa until the mass of the polymer solution became 16.7 kg (polymer concentration: 36% by mass).

[0280] (Prepolymer solution preparation step)

[0281] Then, 1.2 kg of PGME and 7.3 kg of PGMEA were added to dilute the mixture to prepare 25.2 kg of prepolymer solution (polymer concentration: 23.8% by mass, PGMEA:PGME mass ratio = 38:62)

[0282] (Second Concentration Step)

[0283] The prepolymer solution was slowly concentrated using an evaporator at a heat source temperature of 45°C and a reduced pressure of 10 kPa until the mass of the polymer solution reached 14.5 kg. A portion of the obtained polymer solution was collected for analysis, and the result showed that the polymer concentration was 41.3% by mass and the solvent composition (mass ratio) was PGMEA:PGME=51.8:48.2.

[0284] [Example 5]

[0285] (Polymerization process)

[0286] The polymerization and purification were carried out in the same manner as in Example 1 to obtain an ethyl acetate solution of a polymer.

[0287] (Solvent replacement process)

[0288] Then, the replacement solvent was replaced with PGME to perform solvent replacement, and finally a PGME solution having a polymer concentration of 30% by mass and a low boiling point solvent and water content of less than 0.1% each was prepared.

[0289] <Determination of Concentration Ck of Prepolymer Solution and Mass Ratio of PGMEA·PGME>

[0290] The polymer concentration Ck of the prepolymer solution was set to 29 mass %. When the prepolymer solution was concentrated to 50 mass % in the second concentration step, the concentration of the solvent R = (100 - C) / (100 x C / Ck - C) = 0.41.

[0291] A PGMEA / PGME mixed solvent having a PGME composition greater than 30% of the target was prepared in the same manner as in Example 1, and a preliminary test was conducted to investigate the solvent composition ratio when the total mass was reduced to 41% by distillation under the conditions of reduced pressure of 1 kPa and temperature of 45°C. As a result, if a mixed solvent having a PGMEA / PGME mass ratio of 58 / 42 was distilled to a concentration of 41%, the PGMEA / PGME mass ratio became 70 / 30, which is the same value as the target solvent composition. From this result, it is predicted that if the prepolymer solution is adjusted in such a way that the polymer concentration is 29% by mass and the PGMEA / PGME mass ratio is 58 / 42, then when the prepolymer solution is concentrated to a polymer concentration of 50% by mass, a polymer solution having the target polymer concentration and solvent composition can be obtained.

[0292] (First Concentration Step)

[0293] 250 g of the PGME solution having a polymer concentration of 30% by mass obtained in the solvent replacement step was gradually concentrated under the conditions of a heat source temperature of 45° C. and a reduced pressure of 10 kPa to obtain 150 g of a PGME solution having a polymer concentration of 50% by mass.

[0294] (Prepolymer solution preparation step)

[0295] 107 g of PGMEA and 2.0 g of PGME were added to the above solution to dilute it, thereby preparing 259 g of a prepolymer solution having a polymer concentration of 29% by mass and a PGMEA:PGME mass ratio of 58:42.

[0296] (Second Concentration Step)

[0297] The prepolymer solution was added to the flask and slowly concentrated under reduced pressure using an evaporator at a reduced pressure of 10 kPa and a heat source temperature of 45° C. The mass of the flask content at the end of concentration was 139 g, the polymer concentration was 54.1% by mass, and the solvent composition was PGMEA:PGME=66:34.

[0298] (Composition adjustment process)

[0299] 10.5 g of PGMEA and 0.9 g of PGME were added to the above solution, and the mixture was stirred to obtain a polymer solution having a polymer concentration of 50% by mass and a solvent composition of PGMEA:PGME=70:30.

[0300] [Example 6]

[0301] By the same procedure as in Example 5, a PGME solution of a PHS / TBA copolymer having a polymer concentration of 30% by mass and containing a low boiling point solvent and water at contents of less than 0.1% each was prepared.

[0302] <Determination of Concentration Ck of Prepolymer Solution and Mass Ratio of PGMEA·PGME>

[0303] The polymer concentration Ck of the prepolymer solution was set to 39% by mass. When the prepolymer solution was concentrated to 50% by mass in the second concentration step, the concentration of the solvent R=(100-C) / (100×C / Ck-C)=0.64.

[0304] A PGMEA / PGME mixed solvent having a PGME composition greater than 70% of the target was prepared in the same manner as in Example 1, and a preliminary test was conducted to investigate the solvent composition ratio when the total mass was reduced to 64% by distillation under the conditions of reduced pressure of 1 kPa and temperature of 45°C. As a result, if a mixed solvent having a PGMEA / PGME mass ratio of 25 / 75 is distilled to a concentration of 64%, the PGMEA / PGME mass ratio becomes 30 / 70, which is the same value as the target solvent composition. From this result, it is predicted that if the prepolymer solution is adjusted in such a way that the polymer concentration is 39% by mass and the PGMEA / PGME mass ratio is 25 / 75, then when the prepolymer solution is concentrated to a polymer concentration of 50% by mass, a polymer solution having the target polymer concentration and solvent composition can be obtained.

[0305] (First Concentration Step)

[0306] 250 g of the PGME solution having a polymer concentration of 30% by mass obtained in the solvent replacement step was slowly distilled and concentrated to a polymer concentration of 45% by mass under the conditions of a heat source temperature of 45° C. and a reduced pressure of 10 kPa.

[0307] (Prepolymer solution preparation step)

[0308] 31 g of PGMEA was added to the above solution to dilute it, thereby preparing 198 g of a prepolymer solution having a polymer concentration of 38% by mass and a PGMEA:PGME mass ratio of 25:75.

[0309] (Second Concentration Step)

[0310] The prepolymer solution was added to the flask and slowly concentrated under reduced pressure using an evaporator at a reduced pressure of 10 kPa and a heat source temperature of 45° C. The mass of the flask content at the end of concentration was 147 g, the polymer concentration was 51.0% by mass, and the solvent composition was PGMEA:PGME=32:68.

[0311] (Composition adjustment process)

[0312] 3.5 g of PGME was added to the above solution to make fine adjustments, thereby obtaining a polymer solution having a polymer concentration of 50% by mass and a solvent composition of PGMEA:PGME=30.6:69.4.

[0313] [Example 7]

[0314] (Polymerization process)

[0315] The polymerization and purification were carried out in the same manner as in Example 1 to obtain an ethyl acetate solution of a polymer.

[0316] (Solvent replacement process)

[0317] Then, the replacement solvent was replaced with butyl acetate to perform solvent replacement, and finally a butyl acetate solution having a polymer concentration of 30% by mass and a low boiling point solvent and water content of less than 0.1% each was prepared.

[0318] <Determination of Concentration Ck of Prepolymer Solution and Mass Ratio of Butyl Acetate:PGME>

[0319] The polymer concentration Ck of the prepolymer solution was set to 28.6% by mass. When the prepolymer solution was concentrated to 40% by mass in the second concentration step, the concentration of the solvent R = (100-C) / (100×C / Ck-C) = 0.40.

[0320] Since the boiling points of butyl acetate are 126° C. and PGME are 120° C., it is considered that more PGME will be distilled off during distillation, and therefore the mass ratio of butyl acetate / PGME in the prepolymer solution was set to 40 / 60.

[0321] (First Concentration Step)

[0322] 250 g of the butyl acetate solution having a polymer concentration of 30% by mass obtained in the solvent replacement step was slowly distilled and concentrated to a polymer concentration of 50% by mass under the conditions of a heat source temperature of 45° C. and a reduced pressure of 10 kPa.

[0323] (Prepolymer solution preparation step)

[0324] 112 g of PGME was added to the above solution to dilute it, thereby preparing 262 g of a prepolymer solution having a polymer concentration of 28.6% by mass and a mass ratio of butyl acetate:PGME=40:60.

[0325] (Second Concentration Step)

[0326] The prepolymer solution was placed in a flask and slowly concentrated under reduced pressure using an evaporator at a reduced pressure of 10 kPa and a heat source temperature of 45° C. The polymer concentration of the concentrated polymer solution was 46.2% by mass, and the solvent composition was butyl acetate:PGME=48:52. Although the concentration was slightly insufficient, it was estimated that the target composition would be closer if the concentration was further continued.

[0327] [Example 8]

[0328] (Polymerization process)

[0329] The polymerization and purification were carried out in the same manner as in Example 1 to obtain an ethyl acetate solution of a polymer.

[0330] (Solvent replacement process)

[0331] Then, the replacement solvent was replaced with 2-heptanone to perform solvent replacement, and finally a 2-heptanone solution having a polymer concentration of 30% by mass and a low boiling point solvent and water content of less than 0.1% each was prepared.

[0332] <Determination of Concentration Ck of Prepolymer Solution and Mass Ratio of 2-Heptanone·PGME>

[0333] The polymer concentration Ck of the prepolymer solution was set to 28.6% by mass. When the prepolymer solution was concentrated to 40% by mass in the second concentration step, the concentration of the solvent R = (100-C) / (100×C / Ck-C) = 0.40.

[0334] Since the boiling points of 2-heptanone are 151° C. and PGME are 120° C., it is considered that more PGME will be distilled off during distillation, and therefore the mass ratio of 2-heptanone:PGME in the prepolymer solution was set to 40:60.

[0335] (First Concentration Step)

[0336] 250 g of the 2-heptanone solution having a polymer concentration of 30% by mass obtained in the solvent replacement step was slowly distilled and concentrated to a polymer concentration of 50% by mass under the conditions of a heat source temperature of 45° C. and a reduced pressure of 10 kPa.

[0337] (Prepolymer solution preparation step)

[0338] 112 g of PGME was added to the above solution to dilute it, thereby preparing 262 g of a prepolymer solution having a polymer concentration of 28.6% by mass and a 2-heptanone:PGME mass ratio of 40:60.

[0339] (Second Concentration Step)

[0340] The prepolymer solution was placed in a flask and slowly concentrated under reduced pressure using an evaporator at a reduced pressure of 10 kPa and a heat source temperature of 45° C. The polymer concentration of the concentrated polymer solution was 47.8% by mass, and the solvent composition was 2-heptanone:PGME=47:53. Although the concentration was slightly insufficient, it was estimated that the target composition would be closer if the concentration was further continued.

[0341] [Example 9]

[0342] (Polymerization step·Solvent replacement step)

[0343] The polymerization, purification and solvent replacement were carried out in the same manner as in Example 1 to prepare a PGMEA solution having a polymer concentration of 30% by mass and a low boiling point solvent and water content of less than 0.1% each.

[0344] <Determination of Concentration Ck of Prepolymer Solution and Mass Ratio of Dimethylacetamide:PGMEA>

[0345] The polymer concentration Ck of the prepolymer solution is set to 29.0 mass %. When the prepolymer solution is concentrated to 45 mass % in the second concentration step, the concentration of the solvent R=(100-C) / (100×C / Ck-C)=0.50.

[0346] According to the boiling point of dimethylacetamide of 165°C and the boiling point of PGMEA of 146°C, it is believed that PGMEA will be distilled away more during distillation. Therefore, a mixed solvent with a PGMEA composition greater than 50% of the target was prepared, and a preliminary test was conducted to investigate the solvent composition ratio when the overall mass was reduced by 50% under the conditions of reduced pressure of 1 kPa and temperature of 45°C. As a result, if a mixed solvent with a dimethylacetamide:PGMEA mass ratio of 40:60 is distilled to a concentration of 50%, the dimethylacetamide:PGMEA mass ratio obtains a value close to the target 50:50. From this result, it is predicted that if the prepolymer solution is adjusted in a manner such that the polymer concentration is 29% by mass and the mass ratio of PGMEA:PGME is 40:60, then when the prepolymer solution is concentrated to a polymer concentration of 45% by mass, a polymer solution close to the target polymer concentration and solvent composition can be obtained.

[0347] (First Concentration Step)

[0348] 250 g of the PGMEA solution having a polymer concentration of 30% by mass obtained in the solvent replacement step was slowly distilled and concentrated to a polymer concentration of 45% by mass under the conditions of a heat source temperature of 45° C. and a reduced pressure of 10 kPa.

[0349] (Prepolymer solution preparation step)

[0350] 19 g of PGMEA and 73 g of dimethylacetamide were added to the above solution to dilute it, thereby preparing 259 g of a prepolymer solution having a polymer concentration of 29.0% by mass and a dimethylacetamide:PGMEA mass ratio of 40:60.

[0351] (Second Concentration Step)

[0352] The prepolymer solution was added to the flask and slowly concentrated under reduced pressure using an evaporator at a reduced pressure of 6 to 10 kPa and a heat source temperature of 45° C. The polymer concentration of the concentrated polymer solution was 46.3% by mass, and the solvent composition was dimethylacetamide:PGMEA=47:53. Although the concentration was slightly insufficient, it was estimated that the target composition would be closer if the concentration was further continued.

[0353] [Example 10]

[0354] (Polymerization process)

[0355] Equimolar amounts of 4-hydroxyphenyl methacrylate and tert-butyl acrylate were dissolved in a mixed solvent of PGMEA and acetone (mass ratio 70:30), and dimethyl 2,2-azobisisobutyrate was added as a polymerization initiator to prepare a monomer solution.

[0356] A mixed solvent of PGMEA and acetone (mass ratio of 70:30) was added to a reaction vessel equipped with a stirrer, a condenser, and a thermometer, and the mixture was heated to 80°C while stirring. The monomer solution was added dropwise at a constant rate over 4 hours, and the polymerization reaction was further continued for 3 hours, and then cooled to room temperature. The polymerization solution was analyzed by GC, and the conversion rate of the monomer was 99% or more.

[0357] (Solvent replacement process)

[0358] After the polymerization, no precipitation purification was performed. The polymerization liquid was distilled at a heat source temperature of 40°C and under reduced pressure. PGMEA was added while acetone was distilled off, and finally a PGMEA solution with a polymer concentration of 30% by mass and a low-boiling point solvent and water content of less than 0.1% was prepared.

[0359] The properties of the obtained polymer were: 4-hydroxyphenyl methacrylate: tert-butyl acrylate = 50:50, weight average molecular weight (Mw) = 22,500, and molecular weight distribution (Mw / Mn) = 2.4.

[0360] <Determination of Concentration Ck of Prepolymer Solution and Mass Ratio of PGMEA·PGME>

[0361] The target polymer concentration and PGMEA·PGME mixed solvent mass ratio of the polymer solution were the same as those in Example 1. Therefore, the polymer concentration Ck and PGMEA:PGME mass ratio of the prepolymer solution were set to the same values ​​as those in Example 1.

[0362] Using 250 g of the PGMEA solution having a polymer concentration of 30% by mass obtained in the solvent replacement step, the first concentration step, the prepolymer solution preparation step, and the second concentration step were performed in the same manner as in Example 1. The polymer concentration of the polymer solution obtained in the second concentration step was 51.0% by mass, and the solvent composition (mass ratio) was PGMEA:PGME=51.0:49.0.

[0363] (Composition adjustment process)

[0364] To the above solution, 0.9 g of PGMEA and 2.0 g of PGME were added to finely adjust the polymer concentration and the like, and finally a polymer solution having a polymer concentration of 50.0% by mass and a solvent composition of PGMEA:PGME=50.2:49.8 was obtained.

[0365] [Example 11]

[0366] A p-hydroxystyrene homopolymer (MARUKA LYNCUR S2 manufactured by Maruzen Petrochemical, weight average molecular weight (Mw) = 5500, molecular weight distribution (Mw / Mn) = 2.0) was dissolved in ethyl acetate to prepare a solution having a polymer concentration of 15% by mass. The polymer solution was then washed with a 1% by mass aqueous oxalic acid solution and then repeatedly washed with pure water to remove metal impurities.

[0367] For the ethyl acetate solution of the polymer after water washing, PGMEA is added while distilling off ethyl acetate at a heat source temperature of 45°C under reduced pressure, and finally a PGMEA solution is prepared in which the polymer concentration is 30% by mass and the contents of low-boiling point solvents such as the polymerization solvent and the purification solvent and water are each less than 0.1%.

[0368] <Determination of Concentration Ck of Prepolymer Solution and Mass Ratio of PGMEA·PGME>

[0369] The target polymer concentration and PGMEA·PGME mixed solvent mass ratio of the polymer solution were the same as those in Example 1. Therefore, the polymer concentration Ck and PGMEA·PGME mass ratio of the prepolymer solution were set to the same values ​​as those in Example 1.

[0370] Using 250 g of the PGMEA solution having a polymer concentration of 30% by mass obtained in the solvent replacement step, the first concentration step, the prepolymer solution preparation step, and the second concentration step were performed in the same manner as in Example 1. The polymer concentration of the polymer solution obtained in the second concentration step was 53.4% ​​by mass, and the solvent composition was PGMEA:PGME=53.3:46.7.

[0371] (Composition adjustment process)

[0372] To the above solution, 2.5 g of PGMEA and 6.8 g of PGME were added to finely adjust the polymer concentration and the like, and finally a polymer solution having a polymer concentration of 50.1% by mass and a solvent composition of PGMEA:PGME=50.0:50.0 was obtained.

[0373] [Example 12]

[0374] (Polymerization process)

[0375] 4-Hydroxyphenyl methacrylate and tert-butyl acrylate were dissolved in a mixed solvent of PGMEA and acetone (mass ratio: 70:30) at a molar ratio of 10:90, and dimethyl 2,2-azobisisobutyrate was added as a polymerization initiator to prepare a monomer solution.

[0376] A mixed solvent of PGMEA and acetone (mass ratio of 70:30) was added to a reaction vessel equipped with a stirrer, a condenser, and a thermometer, and the mixture was heated to 80°C while stirring. The monomer solution was added dropwise at a constant rate over 4 hours, and the polymerization reaction was further continued for 3 hours, and then cooled to room temperature. The polymerization solution was analyzed by GC, and the conversion rate of the monomer was 99% or more.

[0377] (Solvent replacement process)

[0378] After the polymerization, no precipitation purification was performed. The polymerization liquid was distilled at a heat source temperature of 40°C and under reduced pressure. PGMEA was added while acetone was distilled off, and finally a PGMEA solution with a polymer concentration of 32.8% by mass and a low-boiling point solvent and water content of less than 0.1% was prepared.

[0379] The properties of the obtained polymer were: 4-hydroxyphenyl methacrylate: tert-butyl acrylate = 10:90, weight average molecular weight (Mw) = 21,400, and molecular weight distribution (Mw / Mn) = 2.76.

[0380] <Determination of Concentration Ck of Prepolymer Solution and Mass Ratio of PGMEA·PGME>

[0381] The polymer concentration Ck of the prepolymer solution is set to 40% by mass. When the prepolymer solution is concentrated to 60% by mass in the second concentration step, the concentration of the solvent is R=(100-C) / (100×C / Ck-C)=0.44.

[0382] With reference to Example 1, the solvent composition ratio of the prepolymer solution of Example 12 was estimated as follows. In Example 1, when the solvent composition of the prepolymer solution was set to a mass ratio of PGMEA:PGME = 40:60, the target solvent composition of PGMEA:PGME mass ratio = 50:50 was achieved at a concentration of R = 0.40. In Example 12, R = 0.44, so the ratio of solvent distillation was smaller than that of Example 1, and it can be predicted that the composition changes of PGMEA and PGME were also smaller than that of Example 1. Therefore, the variation range of the solvent composition was estimated to be about 7%, and the mass ratio of the solvent composition of the prepolymer solution was set to 33:67 relative to the target solvent composition of PGMEA:PGME mass ratio = 40:60.

[0383] (First Concentration Step)

[0384] 300 g of the PGMEA solution having a polymer concentration of 32.8% by mass obtained in the solvent replacement step was slowly concentrated using an evaporator at a heat source temperature of 50° C. and a reduced pressure of 1 kPa to obtain 147 g of a PGMEA solution having a polymer concentration of 67.0% by mass.

[0385] (Prepolymer solution preparation step)

[0386] 100 g of PGME was added to the above solution to dilute it, thereby preparing 247 g of a prepolymer solution having a polymer concentration of 39.8% by mass and a PGMEA:PGME mass ratio of 32.7:67.2.

[0387] (Second Concentration Step)

[0388] The prepolymer solution was slowly concentrated under reduced pressure using an evaporator at a reduced pressure of 1 to 10 kPa and a heat source temperature of 50° C. The concentration was completed when the mass of the flask contents reached 164 g. The obtained polymer solution was analyzed, and the polymer concentration was 60.0% by mass, and the solvent composition was PGMEA:PGME=43.5:56.5.

[0389] [Comparative Example 1]

[0390] A method was tried in which a polymer solution with a very high concentration was prepared using PGMEA as a solvent, and PGME was added thereto to prepare a target polymer solution.

[0391] The polymerization, purification and solvent replacement of p-hydroxystyrene and tert-butyl acrylate were carried out in the same manner as in Example 1 to prepare 1 kg of a PGMEA solution having a polymer concentration of 30% by mass and containing low-boiling point solvents such as a polymerization solvent and a purification solvent and water contents of less than 0.1% each.

[0392] In order to make the polymer concentration after PGME addition to be 50% by mass and the mass ratio of PGMEA to PGME to be 50:50, a PGMEA solution with a polymer concentration of 66.7% by mass is required. Therefore, the polymer solution after the solvent replacement is further concentrated at 45°C under reduced pressure. When the concentration is continued until the liquid volume (442g) equivalent to a polymer concentration of about 68% by mass is reached, the precipitation of the polymer is significant. PGMEA8g and PGME150g are added thereto, and stirred to redissolve the precipitated polymer. It took more than 24 hours to redissolve the polymer and make a uniform polymer solution. Although a polymer solution of the target composition was finally obtained, it took a long preparation time and a large amount of high-viscosity solids were precipitated, which indicated that the risk of stopping stirring, failure of the stirring device, etc. was increased.

[0393] [Comparative Example 2]

[0394] The polymerization and purification of p-hydroxystyrene and tert-butyl acrylate were carried out in the same manner as in Example 1 to obtain an ethyl acetate solution of the polymer. The polymer solution was transferred to a tray, and the solvent was evaporated to dryness under the conditions of a reduced pressure of 10 kPa to 1 kPa and a temperature of 50° C. to obtain a polymer powder. It took more than 24 hours to reduce the ethyl acetate concentration contained in the polymer to less than 1% by mass.

[0395] In order to prepare a polymer solution of the target composition, 700 g of PGMEA and 300 g of PGME were added to 1 kg of the polymer powder and stirred. However, even after stirring for more than 1 hour, the polymer was not completely redissolved.

[0396] Industrial Applicability

[0397] The present invention can be used to prepare a resist polymer solution suitable for preparing a resist composition, especially a resist composition for a thick film.

Claims

1. A method for producing a polymer solution, characterized in that: A method for manufacturing a polymer solution containing C mass% of a polymer in a mixed solvent obtained by mixing at least two or more solvents in a specified mass ratio. The manufacturing method includes the following steps: First concentration step: A step of concentrating a solution obtained by dissolving the polymer in at least one solvent in the mixed solvent so that the polymer concentration becomes Cz (0.8C < Cz ≤ C + 10) mass%. Prepolymer solution preparation step: A step of adding a solvent for the mixed solvent to the polymer solution obtained in the first concentration step to prepare a prepolymer solution. In this step, The prepolymer solution is a solution containing Cz (0.3C ≤ Cz ≤ 0.8C) mass% of the polymer in the mixed solvent, and is a solution in which the mass ratio of at least two or more solvents in the mixed solvent becomes ±5% of the specified mass ratio when the prepolymer solution is concentrated from the polymer concentration Cz mass% to C mass%. And Second concentration step: A step of concentrating the prepolymer solution to a polymer concentration of C mass%.

2. The method for producing a polymer solution according to claim 1, wherein: The mass ratio of each solvent in the prepolymer solution is obtained by the following preliminary test. (Steps of the preliminary test) Set the polymer concentration of the prepolymer solution to Cz mass%; calculate the concentration degree R of the solvent when the prepolymer solution is concentrated to a polymer concentration of C mass% in the second concentration step {R = (100 - C) / (100×C / Cz - C)}. Next, prepare a mixed solvent in which the composition of the solvent that is considered to be largely distilled off during distillation according to the boiling point and vapor pressure of each solvent is more than the target composition, perform distillation until the total mass of the mixed solvent is reduced to the value obtained by multiplying it by the concentration degree R, and obtain the solvent composition ratio after distillation; obtain the mixed solvent composition ratio at which the solvent composition ratio after distillation becomes equal to the target composition, and use this mixed solvent composition ratio as the mass ratio of each solvent in the prepolymer solution.

3. The method for producing a polymer solution according to claim 1 or 2, wherein: Before the first concentration step, there is also a solvent replacement step: a step of reducing low-boiling impurities other than this solvent by performing distillation under reduced pressure while adding at least one solvent in the mixed solvent to the solution containing the polymer.

4. The method for producing a polymer solution according to claim 1 or 2, wherein: After the second concentration step, there is also a composition adjustment step: a step of adding a solvent to the polymer solution to adjust the polymer concentration and the mixed solvent composition.

5. The method for producing a polymer solution according to claim 1 or 2, wherein: The polymer concentration C in the polymer solution is 30 to 70 mass%.

6. The method for producing a polymer solution according to claim 1 or 2, wherein: Relative to the total mass of the mixed solvent of the polymer solution, the concentration of the first solvent is 45 mass% or more and less than 80 mass%, and the concentration of the second solvent is 20 mass% or more and 50 mass% or less.

7. The method for producing a polymer solution according to claim 1 or 2, wherein: The polymer is a polymer for resist, and the mixed solvent is a solvent for resist.

Citation Information

Patent Citations

  • Polymer solution for resist and method for preparing same

    JP2005173252A

  • Method for producing polymer solution for arf excimer laser resist

    JP2006161052A

  • Manufacturing method of photoresist resin solution

    JP2006176574A

  • Heat dissipation film, and production method and apparatus therefor

    JP2014127518A

  • Chemically amplified positive resist dry film, dry film laminate and production method of the same

    JP2019105847A