Composite membrane as well as preparation method and application thereof
By loading cerium hydroxide nanoparticles on the fiber membrane, the problem of low removal efficiency of trace phosphate in water is solved, efficient and environmentally friendly phosphate adsorption effect is achieved, and a recyclable solution is provided.
Patent Information
- Application Number
- CN202411105213.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is inefficient when removing trace phosphate in water, and traditional methods have high costs, sludge generation and biosafety problems. The preparation process of nanocomposites is complex and the physical and chemical properties are unpredictable.
Electrosparks were prepared by electrospark ablation method and loaded to the surface of the fiber membrane. By ionization, cerium ions were formed to bind to phosphate ions to form water-insoluble cerium phosphate, thereby improving the adsorption effect of phosphate.
It has achieved efficient adsorption of phosphate, with a maximum adsorption capacity of 95.2mg P/g, and the preparation method is simple and environmentally friendly. The material can be recycled and adapted to different pH environments.
Smart Images

Figure CN118988009A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of membrane materials, and in particular relates to a composite membrane and a preparation method and application thereof. Background Art
[0002] Phosphate is an important nutrient for biological growth in ecosystems and a key factor in causing lake eutrophication. When phosphorus levels are too high, algal blooms may occur, the main feature of which is the excessive growth of blue-green algae as the dominant species, competing with aquatic organisms for oxygen and sunlight. In addition, blue-green algae release algal toxins, which cause lethal or sublethal effects on organisms, ultimately leading to a decrease in the number of aquatic organisms and a decrease in dissolved oxygen levels in the water. This will threaten the health of the ecosystem and lead to global water pollution problems. Strictly controlling the phosphorus content in water bodies is a key step in curbing lake eutrophication and maintaining the health of aquatic ecosystems, so it is particularly important to develop efficient dephosphorization technology.
[0003] Chemical precipitation, biological treatment and adsorption are commonly used phosphorus removal technologies. Chemical precipitation mainly involves adding cationic salts, such as calcium and magnesium, so that metal salts react with dissolved phosphorus to form insoluble phosphates and precipitate. Although chemical precipitation is commonly used in wastewater phosphorus removal in the chemical industry, the consumption of a large amount of chemical reagents and the cost of sludge treatment are high. Biological treatment methods often achieve the corresponding treatment effect by accumulating phosphorus in cells through polyphosphate microorganisms (including certain harmful microorganisms), but there are certain biosafety issues and sludge is also produced. Traditional chemical precipitation and biological treatment technologies are difficult to remove trace amounts of phosphorus in water bodies, and the treatment effects are gradually unable to meet the increasingly stringent phosphorus removal regulations. In contrast, the adsorption method has the characteristics of less sludge production, simple operation, and reusability. It can treat water bodies containing trace phosphorus (below 0.5 mg / L) and is effective in controlling phosphates.
[0004] Cerium (Ce) is an abundant and inexpensive rare earth element that is non-toxic or low-toxic to the human body. The smaller ionic potential makes cerium show good potential for the removal of anionic pollutants such as phosphate, arsenate and fluoride. At present, the synthesis of cerium-containing nanocomposites is mostly carried out by impregnation to load cerium onto the matrix material. In this wet chemical process, the chemical precursors used in the synthesis process may contaminate the nanomaterials, and harmful residues and by-product wastes also need to be handled in a friendly manner. Moreover, nanoparticles are limited by slow kinetics and operation, the changes in physicochemical properties are unpredictable, and the resulting membrane materials have poor adsorption effects on phosphates. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a composite membrane and a preparation method and application thereof. The composite membrane prepared by the present invention has good adsorption effect on phosphate and high adsorption capacity.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a composite membrane, comprising a fiber membrane and cerium hydroxide nanoparticles loaded on the fiber surface of the fiber membrane;
[0008] The fiber membrane includes one or more of cellulose acetate membrane, chitosan fiber membrane, polyacrylonitrile fiber membrane, polystyrene fiber membrane and polyvinylidene fluoride fiber membrane.
[0009] Preferably, the particle size of the cerium hydroxide nanoparticles is 200-300 nm, and the loading amount of the cerium hydroxide nanoparticles on the composite membrane is 10%-20%.
[0010] The present invention also provides a method for preparing the composite film described in the above technical solution, comprising the following steps:
[0011] The metal cerium is processed by electric spark ablation to obtain cerium nanoparticles;
[0012] The cerium nanoparticles are oxidized and mixed with alkaline steam, and the obtained aerosol is deposited on the surface of the fiber membrane to obtain an alkaline fiber membrane containing cerium oxide;
[0013] The cerium oxide-containing alkaline fiber membrane is subjected to a hydration reaction to obtain a composite membrane.
[0014] Preferably, the electric spark ablation occurs in a nanoparticle generator, and the parameters of the nanoparticle generator include: voltage of 0.96-1.42 kV, current of 9.0-9.8 mA, metal cerium as the counter electrode, and an electrode spacing of 5-15 mm.
[0015] Preferably, the nanoparticle generator uses an oxygen-containing mixed gas as a carrier gas, and the volume fraction of oxygen in the oxygen-containing mixed gas is 1-4%.
[0016] Preferably, the alkaline steam is steam of an ammonia solution, and the volume fraction of the ammonia solution is 15% to saturated ammonia water.
[0017] Preferably, the deposition time is 20 to 50 minutes.
[0018] Preferably, the fiber membrane is a polyacrylonitrile fiber membrane, the fiber diameter of the polyacrylonitrile fiber membrane is 1 to 1.5 μm, and the porosity is 70% to 90%.
[0019] Preferably, the hydration reaction is carried out at a temperature of 100 to 150° C. and for a time of 4 to 9 hours.
[0020] The present invention also provides the use of the composite membrane described in the above technical solution or the composite membrane obtained by the above preparation method in adsorbing phosphate.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention provides a composite membrane, comprising a fiber membrane and cerium hydroxide nanoparticles loaded on the fiber surface of the fiber membrane; the fiber membrane comprises one or more of cellulose acetate membrane, chitosan fiber membrane, polyacrylonitrile fiber membrane, polystyrene fiber membrane and polyvinylidene fluoride fiber membrane.
[0023] The present invention uses a fiber membrane of a specific material type, and the fiber structure can reduce the aggregation of nanoparticles, improve the uniformity of the distribution of cerium hydroxide nanoparticles, and the surface particles have a good degree of bonding with the fiber; the cerium hydroxide nanoparticles loaded on the fiber surface of the fiber membrane are ionized to form cerium ions, and the cerium ions and phosphate ions form water-insoluble cerium phosphate, thereby achieving the effect of removing phosphate. In the composite membrane material prepared by the present invention, the cerium hydroxide nanoparticles are evenly distributed on the surface of the spinning fiber, which can improve the collision and bonding of the active adsorption sites with phosphate, thereby improving the overall adsorption performance of the composite membrane and improving the adsorption rate of the membrane material to phosphate. The results of the embodiment show that the composite membrane of the present invention can efficiently capture phosphate, and the maximum adsorption capacity reaches 95.2 mg P / g.
[0024] The present invention also provides a method for preparing the composite film described in the above technical scheme. The present invention adopts electric spark ablation technology to prepare nanoparticles, and does not need to use any chemical reagents. The preparation method is simple, rapid, green, efficient and environmentally friendly. The formed nanoaerosol is then subjected to deposition and hydration treatment to prepare the composite film. The operation is simple and easy. The nanoaerosol is stable and cerium hydroxide is formed after hydration. The changes in physical and chemical properties are predictable. Only simple precursor materials are needed to efficiently produce the composite film, which provides the possibility for future industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 is a scanning electron microscope image of the composite film prepared in Example 1;
[0027] Figure 2 This is a graph showing the relationship between the adsorption capacity and time of the composite membrane prepared in Example 1;
[0028] Figure 3 This is a graph showing the removal results of the composite membrane prepared in Example 1 after being recycled 4 times to adsorb phosphate solution;
[0029] Figure 4 The adsorption capacity of the composite membrane prepared in Example 1 when used in environments with different pH values. DETAILED DESCRIPTION
[0030] The present invention provides a composite membrane, comprising a fiber membrane and cerium hydroxide nanoparticles loaded on the fiber surface of the fiber membrane;
[0031] The fiber membrane includes one or more of cellulose acetate membrane, chitosan fiber membrane, polyacrylonitrile fiber membrane, polystyrene fiber membrane and polyvinylidene fluoride fiber membrane.
[0032] In the present invention, the particle size of the cerium hydroxide nanoparticles is preferably 200-300 nm, and the loading amount of the cerium hydroxide nanoparticles on the composite membrane is preferably 10%-20%, more preferably 15%-17%.
[0033] The present invention also provides a method for preparing the composite film described in the above technical solution, comprising the following steps:
[0034] The metal cerium is processed by electric spark ablation to obtain cerium nanoparticles;
[0035] The cerium nanoparticles are oxidized and mixed with alkaline steam, and the obtained aerosol is deposited on the surface of the fiber membrane to obtain an alkaline fiber membrane containing cerium oxide;
[0036] The cerium oxide-containing alkaline fiber membrane is subjected to a hydration reaction to obtain a composite membrane.
[0037] In the present invention, unless otherwise specified, the materials and equipment used are commercially available products in the art.
[0038] The invention processes metal cerium by electric spark ablation to obtain cerium nanoparticles; oxidizes the cerium nanoparticles and mixes them with alkaline steam, and deposits the obtained aerosol on the surface of a fiber membrane to obtain an alkaline fiber membrane containing cerium oxide.
[0039] In the present invention, the electric spark ablation preferably occurs in a nanoparticle generator, such as VSP-G1. The parameters of the nanoparticle generator include: the voltage is preferably 0.96-1.42 kV, more preferably 1.35-1.42 kV, and more preferably 1.38 kV; the current is preferably 9.0-9.8 mA, more preferably 9.1-9.6 mA, and more preferably 9.5 mA; with metal cerium as the counter electrode, the electrode spacing is preferably 5-15 mm, and more preferably 10 mm.
[0040] In the present invention, the specification of the metal cerium is preferably 6S, with a purity of 99.99%.
[0041] In the present invention, the nanoparticle generator preferably uses an oxygen-containing mixed gas as a carrier gas, and the volume fraction of oxygen in the oxygen-containing mixed gas is preferably 1% to 4%, and more preferably 2%; the oxygen-containing mixed gas preferably also includes nitrogen or argon, and more preferably argon; the flow rate of the carrier gas is preferably 1 to 5 mL / min, more preferably 3 to 4 mL / min, and more preferably 3.5 mL / min. The present invention uses an oxygen-containing mixed gas as a carrier gas to oxidize the generated cerium nanoparticles in the reaction chamber of the nanoparticle generator to generate cerium oxide nanoparticles.
[0042] In the present invention, the alkaline steam is preferably steam of an ammonia solution, and the volume fraction of the ammonia solution is preferably 15% to saturated ammonia water.
[0043] In the present invention, the proportion of cerium oxide nanoparticles in the aerosol is preferably 13% to 20%.
[0044] In the present invention, an ammonia solution is preferably injected into the bypass pipe of the nanoparticle generator to form alkaline steam; the bypass pipe is located in the rear section of the reaction chamber, and the distance between the bypass pipe and the deposition point is preferably 30 cm; the temperature of the ammonia solution is preferably 38-40° C. The alkaline steam provides an alkaline environment for the subsequent hydration reaction.
[0045] In the present invention, the fiber membrane is preferably an electrospinning membrane.
[0046] In the present invention, the fiber membrane is preferably a polyacrylonitrile fiber membrane, the fiber diameter of the polyacrylonitrile fiber membrane is preferably 1-1.5 μm, the porosity is preferably 70%-90%, and more preferably 75%-80%. The composite membrane made of the polyacrylonitrile fiber electrospinning membrane described in the present invention has high phosphate removal efficiency (good adsorption performance) and can be recycled many times (good stability).
[0047] In the present invention, the deposition time is preferably 20 to 50 minutes, more preferably 30 to 40 minutes. The cerium oxide preferably covers 90% of the fiber membrane area.
[0048] In the present invention, the fiber membrane is preferably placed in a deposition component of a nanoparticle generator for deposition. The deposition component preferably uses a VSP-A2 deposition accessory. The deposition chamber is more spacious, which is conducive to uniform distribution of airflow. On the one hand, it can increase the loading amount of cerium oxide nanoparticles on the electrospinning membrane, and on the other hand, it can further improve the uniformity of the distribution of cerium oxide nanoparticles, thereby significantly improving the adsorption efficiency.
[0049] After obtaining the cerium oxide-containing alkaline fiber membrane, the present invention performs a hydration reaction on the cerium oxide-containing alkaline fiber membrane to obtain a composite membrane.
[0050] In the present invention, the hydration reaction is preferably carried out in a high pressure reactor, the temperature of the hydration reaction is preferably 100-150°C, more preferably 110-130°C, and more preferably 115-120°C; the time is preferably 4-9h, more preferably 5-7h, and more preferably 6h. During the hydration reaction, the cerium oxide nanoparticles are hydrated to generate cerium hydroxide nanoparticles.
[0051] In the present invention, the hydration reaction preferably further includes drying, and the drying temperature is preferably 55 to 60° C., and the drying time is preferably 12 to 13 hours.
[0052] In the present invention, the porosity of the composite membrane is preferably 70% to 80%.
[0053] The present invention also provides the use of the composite membrane described in the above technical solution or the composite membrane obtained by the above preparation method in adsorbing phosphate.
[0054] In the present invention, the phosphate is preferably the phosphate in water, and the concentration of the phosphate in the water is preferably 30 mg / L.
[0055] The composite membrane prepared by the invention can efficiently adsorb phosphate in water, the maximum adsorption capacity of phosphorus reaches 95.2 mg P / g, the adsorption effect is good, the growth of green algae can be inhibited, and algal bloom can be prevented.
[0056] In the present invention, after the composite membrane adsorbs phosphate, it is preferred that the composite membrane adsorbed with phosphate further comprises: regenerating (desorbing) the composite membrane adsorbed with phosphate; the regeneration method preferably comprises: soaking the composite membrane adsorbed with phosphate in a sodium chloride-sodium hydroxide mixture, washing, and drying to obtain a regenerated composite membrane. The regenerated composite membrane can be reused. During the adsorption process, cerium hydroxide and phosphate form cerium phosphate, thereby removing phosphate from the water body; the composite membrane adsorbed with phosphate is soaked in a sodium chloride-sodium hydroxide mixture, the phosphate is dissolved and ionized, and then eluted from the composite membrane.
[0057] The total concentration of the sodium chloride-sodium hydroxide mixed solution is preferably 3 mol / L, and the molar ratio of sodium chloride to sodium hydroxide in the mixed solution is preferably 1:1; the soaking time is preferably 12 hours; the washing reagent is preferably water; the drying temperature is preferably 40° C., and the drying time is preferably 2 hours.
[0058] The composite membrane prepared by the invention can be washed and regenerated by alkali solution and can be reused many times, which is beneficial to saving economic cost.
[0059] In order to further illustrate the present invention, the composite membrane provided by the present invention and its preparation method and application are described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.
[0060] Example 1
[0061] The preparation of the electrospinning membrane containing cerium comprises the following steps:
[0062] (1) A polyvinylidene fluoride spinning membrane is selected as a carrier, the fiber diameter is 1 to 1.5 μm, and the porosity is 80%.
[0063] (2) A pair of cerium electrodes with an electrode spacing of 10 mm were selected and inserted into both ends of the VSP-G1 instrument (nanoparticle generator). An upgraded version of the VSP-A2 deposition accessory that can achieve higher yields was used (the movement distance of the particles in the chamber becomes shorter and the nanoparticle yield is high). The VSP-G1 instrument parameters were set to 1.38 kV and 9.6 mA. The carrier gas was a 4% O2 + 96% Ar mixture with a flow rate of 3 L / min passing vertically through the cerium electrodes. A saturated ammonia flow at 40°C was injected into the bypass pipe of the reaction chamber. The obtained cerium-containing nanoparticles were deposited on the polyvinylidene fluoride spinning membrane for 30 min.
[0064] (3) The material obtained in step (2) was placed in a reaction kettle for hydration at 130° C. for 7 h, and then the membrane was taken out and placed in an oven at 60° C. for drying to obtain a composite membrane.
[0065] The composite membrane (adsorbent material) obtained in Example 1 has a surface morphology as shown in Figure 1 As shown in the figure, the scale is 15μm, and it can be seen that the cerium hydroxide nanoparticles are successfully loaded on the fiber surface of the membrane material. The particle size of the cerium hydroxide nanoparticles on the composite membrane is 200-300nm, and the loading amount is 15%.
[0066] Application Example 1
[0067] The composite membrane prepared in Example 1 was used to remove phosphate in water, and the usage ratio of the composite membrane to the water was 0.1 g:500 mL:
[0068] Adsorption experiments were carried out in simulated water containing 30 mg / L phosphate (potassium dihydrogen phosphate) and a pH value of 7. Figure 2 This is a test result graph of the relationship between the adsorption capacity and time of the cerium-containing fiber membrane prepared in Example 1; the adsorbent reaches adsorption equilibrium after about 700 minutes of adsorption at room temperature, and the adsorption capacity is calculated by simulating the concentration change before and after adsorption, the volume of the water body and the added mass of the composite membrane, and its maximum adsorption capacity is 86.7 mg / g.
[0069] Figure 3 The figure is a graph showing the removal results of phosphate solution adsorbed by the cerium-containing fiber membrane prepared in Example 1 after four cycles. The adsorption-desorption experiment was repeated four times, and the phosphate removal efficiencies were 72.5%, 64.3%, 61.4% and 57.5%, respectively.
[0070] Steps for composite membrane elution regeneration (desorption):
[0071] The composite membrane was immersed in 50 mL of 3 mol / L sodium chloride-sodium hydroxide solution (sodium chloride-sodium hydroxide molar ratio 1:1) at room temperature for 12 h; then washed with deionized water until neutral, and dried in a drying oven at 40° C. for 2 h.
[0072] In the elution regeneration step, the composite membrane is soaked in a 3 mol / L sodium chloride-sodium hydroxide solution, and the phosphate on the membrane adsorbent is recovered into the solution. The obtained phosphate-rich soaking solution is adjusted to neutral with hydrochloric acid to achieve the recovery and utilization of the phosphate.
[0073] Figure 4 The adsorption capacity of the cerium-containing fiber membrane prepared in Example 1 when used in different pH environments. The composite membrane prepared in the present invention has a wide pH adaptability range and can cope with the removal of phosphates in different environments.
[0074] Example 2
[0075] The preparation of the electrospinning membrane containing cerium comprises the following steps:
[0076] (1) Chitosan spinning membrane was selected as the carrier.
[0077] (2) A pair of cerium electrodes were inserted into both ends of the VSP-G1 instrument. The upgraded VSP-A2 deposition accessory was used. The VSP-G1 instrument parameters were set to 1.35 kV and 9.1 mA. The carrier gas was a 4% O2 + 96% Ar mixture with a flow rate of 5 L / min passing vertically through the electrode target. A saturated ammonia flow at 40°C was injected into the bypass pipe of the reaction chamber. The obtained cerium-containing nanoparticles were deposited on the chitosan spinning membrane for 30 minutes.
[0078] (3) The material obtained in step (2) was placed in a reaction kettle for hydration at 110° C. for 6 h, and then the membrane was taken out and placed in an oven at 60° C. for drying to obtain a composite membrane. The loading amount of cerium hydroxide nanoparticles on the composite membrane was 17%.
[0079] The composite membrane prepared in Example 2 was placed in a simulated water body with a concentration of 30 mg / L for adsorption experiment. After 500 minutes of adsorption, the adsorbent reached adsorption equilibrium, and the maximum adsorption capacity was 91.7 mg / g.
[0080] The process was repeated 4 times, and the phosphate removal efficiency at the fourth time was 56.3%.
[0081] Example 3
[0082] The preparation of the electrospinning membrane containing cerium comprises the following steps:
[0083] (1) Use acetate fiber spinning membrane as the carrier.
[0084] (2) A pair of cerium electrodes were inserted into both ends of the VSP-G1 instrument. The upgraded VSP-A2 deposition accessory was used. The VSP-G1 instrument parameters were set to 1.35 kV and 9.1 mA. The carrier gas was a mixture of 2% O2 + 98% Ar with a flow rate of 2.5 L / min passing vertically through the electrode target. A saturated ammonia flow at 38°C was injected into the bypass pipe of the reaction chamber. The obtained cerium-containing nanoparticles were deposited on the acetate fiber spinning membrane for 30 minutes.
[0085] (3) The material obtained in step (2) was placed in a reaction kettle for hydration at 120° C. for 4 h, and then the membrane was taken out and placed in an oven at 55° C. for drying to obtain a composite membrane. The loading amount of cerium hydroxide nanoparticles on the composite membrane was 13%.
[0086] The composite membrane prepared in Example 3 was placed in a simulated water body with a concentration of 30 mg / L for adsorption experiment. After 500 minutes of adsorption, the adsorbent reached adsorption equilibrium, and the maximum adsorption capacity was 72.3 mg / g.
[0087] After 4 repetitions, the phosphate removal efficiency was 58.6%.
[0088] Example 4
[0089] The preparation of the electrospinning membrane containing cerium comprises the following steps:
[0090] (1) Polystyrene spinning membrane is selected as the carrier.
[0091] (2) A pair of cerium electrodes were inserted into both ends of the VSP-G1 instrument. The upgraded VSP-A2 deposition accessory was used. The VSP-G1 instrument parameters were set to 1.35 kV and 9.1 mA. The carrier gas was a mixture of 1% O2 + 99% Ar with a volume fraction of 3 L / min passing vertically through the electrode target. A saturated ammonia flow at 40°C was injected into the bypass pipe of the reaction chamber. The obtained cerium-containing nanoparticles were deposited on the polystyrene spinning membrane for 20 minutes.
[0092] (3) The material obtained in step (2) was placed in a reaction vessel at 115° C. for hydration for 5 h, and then the membrane was taken out and placed in an oven at 60° C. for drying to obtain a composite membrane. The loading amount of cerium hydroxide nanoparticles on the composite membrane was 12%.
[0093] The composite membrane prepared in Example 4 was placed in a simulated water body with a concentration of 30 mg / L for adsorption experiment. After 500 minutes of adsorption, the adsorbent reached adsorption equilibrium, and the maximum adsorption capacity was 68.4 mg / g.
[0094] The process was repeated 4 times, and the phosphate removal efficiency at the fourth time was 59.3%.
[0095] Example 5
[0096] The preparation of the electrospinning membrane containing cerium comprises the following steps:
[0097] (1) Polyacrylonitrile membrane is selected as the carrier.
[0098] (2) A pair of cerium electrodes were inserted into both ends of the VSP-G1 instrument. The upgraded VSP-A2 deposition accessory was used. The VSP-G1 instrument parameters were set to 1.42 kV and 9.5 mA. The carrier gas was a 4% O2 + 96% Ar mixed gas that passed vertically through the electrode target at a flow rate of 4 L / min. A saturated ammonia flow at 40°C was injected into the bypass of the reaction chamber. The obtained cerium-containing nanoparticles were deposited on the polyacrylonitrile film for 40 minutes.
[0099] (3) The material obtained in step (2) was placed in a reaction kettle for hydration at 120° C. for 6 h, and then the membrane was taken out and placed in an oven at 60° C. for drying to obtain a composite membrane. The loading amount of cerium hydroxide nanoparticles on the composite membrane was 16%.
[0100] The composite membrane prepared in Example 5 was placed in a simulated water body with a concentration of 30 mg / L for batch adsorption experiments. After 500 minutes of adsorption, the adsorbent reached adsorption equilibrium, and the maximum adsorption capacity was 95.2 mg / g.
[0101] Comparative Example 1
[0102] The difference from Example 5 is that a polyvinyl alcohol electrospinning membrane (fiber diameter 0.6-1.0 μm, porosity 72%) is selected, and the remaining steps are the same as those in Example 5.
[0103] The prepared composite membrane was used to adsorb phosphorus in simulated water. Specifically, 0.1 g of the composite membrane was put into 100 mL of simulated water with a P concentration of 30 mg / L. After adsorption for 3 hours, the P concentration was measured using an inductively coupled plasma mass spectrometer (ICP-MS). The adsorption capacity of the adsorption fiber membrane was 56 mg P / g and remained unchanged.
[0104] It can be seen that the saturated adsorption capacity of cerium deposited on the polyvinyl alcohol electrospun membrane is significantly smaller than that of cerium deposited on the polyacrylonitrile membrane in Example 5, and the surface particle bonding degree of the composite membrane in Example 5 is better.
[0105] Although the above-mentioned embodiments have made a detailed description of the present invention, they are only some embodiments of the present invention, rather than all embodiments. People can also obtain other embodiments based on the embodiments of the present invention without creative work, and these embodiments all fall within the scope of protection of the present invention.
Claims
1. A composite film, characterized in that It comprises a fiber membrane and cerium hydroxide nanoparticles loaded on the fiber surface of the fiber membrane; The fiber membrane includes one or more of cellulose acetate membrane, chitosan fiber membrane, polyacrylonitrile fiber membrane, polystyrene fiber membrane and polyvinylidene fluoride fiber membrane.
2. The composite membrane according to claim 1, characterized in that The particle size of the cerium hydroxide nanoparticles is 200-300nm, and the loading amount of the cerium hydroxide nanoparticles on the composite membrane is 10%-20%.
3. The method for preparing the composite film according to claim 1 or 2, characterized in that: The following steps are involved: The metal cerium is processed by electric spark ablation to obtain cerium nanoparticles; The cerium nanoparticles are oxidized and mixed with alkaline steam, and the obtained aerosol is deposited on the surface of the fiber membrane to obtain an alkaline fiber membrane containing cerium oxide; The cerium oxide-containing alkaline fiber membrane is subjected to a hydration reaction to obtain a composite membrane.
4. The preparation method according to claim 3, characterized in that: The electric spark ablation occurs in a nanoparticle generator, and the parameters of the nanoparticle generator include: voltage of 0.96-1.42 kV, current of 9.0-9.8 mA, metal cerium as a counter electrode, and an electrode spacing of 5-15 mm.
5. The preparation method according to claim 4, characterized in that: The nanoparticle generator uses oxygen-containing mixed gas as carrier gas, and the volume fraction of oxygen in the oxygen-containing mixed gas is 1-4%.
6. The preparation method according to claim 3 or 5, characterized in that: The alkaline steam is steam of an ammonia solution, and the volume fraction of the ammonia solution is 15% to saturated ammonia water.
7. The preparation method according to claim 3 or 5, characterized in that: The deposition time is 20 to 50 minutes.
8. The preparation method according to claim 3, characterized in that: The fiber membrane is a polyacrylonitrile fiber membrane, the fiber diameter of the polyacrylonitrile fiber membrane is 1-1.5 μm, and the porosity is 70%-90%.
9. The preparation method according to claim 3, characterized in that: The temperature of the hydration reaction is 100-150° C., and the time is 4-9 hours.
10. Use of the composite membrane according to claim 1 or 2 or the composite membrane obtained by the preparation method according to any one of claims 3 to 8 in adsorbing phosphate.
Citation Information
Cited By
Method for obtaining colloidal nanosized cerium particles by femtosecond laser ablation
RU2848812C1