Preparation method of crown-embedded ether montmorillonite capable of selectively adsorbing lithium
By embedding 12-crown ether-4 in montmorillonite, the modified adsorbent was formed, and the problem of poor lithium ion adsorption in Bayer method was solved, efficient and highly selective lithium ion adsorption was achieved, and lithium resources were improved. Recovery rate and maintain the stability and low cost characteristics of the process.
Patent Information
- Application Number
- CN202411059169.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-03
- Publication Date
- 2024-11-22
AI Technical Summary
During the Bayer alumina production process, lithium ions are difficult to efficiently selectively adsorption and recovery in sodium aluminate solution, resulting in the failure of effective utilization of lithium resources and affecting the melting point of the subsequent electrolysis process and the solubility of alumina.
By embedding 12-crown ether-4 into the layered structure of montmorillonite, the macrocyclic structure is used to coordinate with lithium ions to form a tetrahedral structure, which realizes the specific capture of lithium ions, and improves the lithium ions Selective adsorption capability. The method includes drying, grinding, ultrasonic dispersion, mixing with 12-crown ether-4, centrifugal washing and freeze-drying to form modified montmorillonite embedded with 12-crown ether-4 as an adsorbent , and selective adsorption of lithium ions is carried out in sodium aluminate solution.
It realizes efficient and selective adsorption of lithium ions, improves the recovery rate of lithium ions, maintains the structural stability of the adsorbent, avoids the introduction of impurities, and is suitable for Bayer method system without changing the original alumina production process. It has the advantages of recycling and low cost.
Smart Images

Figure CN118988246A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adsorption materials, and specifically designs a method for preparing a material for selectively adsorbing and recovering lithium ions in a sodium aluminate solution. Background Art
[0002] China is rich in bauxite resources, which are mainly distributed in Guangxi, Guizhou, Henan, Shanxi, Chongqing, Yunnan and other places. Among them, the bauxite deposits in Henan, Shanxi, Guizhou and other places are generally associated with high content of lithium, which is a potential type of lithium ore resource. The associated lithium resources have great potential for utilization. In the process of extracting the main element aluminum from bauxite (Bayer process alumina production), the layered aluminum silicate minerals (kaolinite, illite, chlorite, montmorillonite, etc.) in bauxite are heated to high temperature (≥260℃) and high alkali concentration (N k ≥240g / L) dissolution conditions, the structure is destroyed, about 80% of the lithium in the mineral lattice and interlayer enters the solution, 20% is discharged with red mud, and the lithium entering the Bayer mother liquor (sodium aluminate solution) finally enters the finished alumina in the form of impurities through processes such as seed decomposition and roasting. The Li2O content in alumina products of several major alumina companies in central my country is above 0.11%, and the Li2O content of imported alumina is usually only 0.006%. If estimated at 0.1%, the output of domestic ore alumina is about 20 million tons / year, and the Li2O taken away by metallurgical grade alumina is as high as 20,000 tons per year. These lithium resources have not been reasonably utilized. What's more, the long-term use of lithium-rich alumina as a raw material will reduce the melting point of the electrolyte and the solubility of alumina in the subsequent electrolysis process. Therefore, the problem of reducing the excessive lithium content in metallurgical grade alumina needs to be solved urgently.
[0003] At present, bauxite-associated lithium resources, as a new type of lithium resource, have received less attention. Research on the utilization of associated lithium resources in bauxite is mainly divided into two categories: direct ore extraction and mother liquor extraction. Direct ore extraction is to directly regard bauxite with a higher lithium grade as a lithium ore raw material, and extract lithium from it through flotation, roasting, acid leaching and other processes. Wu Guobao and others invented "a method for extracting lithium from clay-type lithium ore and a method for preparing lithium aluminate, application number: CN202210866437.8". Clay-type lithium ore, sodium bicarbonate and water are prepared into raw ore slurry, and the raw ore slurry is leached and solid-liquid separated to obtain solid slag and lithium-containing leaching solution, and the lithium leaching rate can reach up to 92%. Xu Xinyu and others invented "a method for extracting lithium from lithium-containing ores, application number: CN202211449279.2". This method activates lithium ore with hydrochloric acid at 45-60 ° C to obtain a lithium-containing acidified liquid, and obtains a lithium-containing concentrated liquid after filtration, nanofiltration and ion exchange. The lithium-containing concentrated liquid is treated with sodium removal to obtain a lithium chloride product. The method has a high lithium yield, and the method does not require high-temperature roasting. In order to extract lithium from low-grade minerals, Du Wuxing and others invented "a method for comprehensive utilization of medium- and low-grade bauxite containing lithium, application number: CN202311232302.7". The medium- and low-grade bauxite is subjected to pre-selection and classification, and the coarse-grained materials are subjected to multiple grinding, gravity treatment, and magnetic separation to obtain high-quality aluminum concentrate and products. Fine-grained materials and tailings can be subjected to magnetic separation to obtain lithium-rich concentrate. This method can fully recover and utilize the valuable components in lithium-containing medium- and low-grade bauxite.
[0004] Salt lake brine is widely distributed and contains rich lithium and other miscellaneous cations. Extracting lithium from it requires good selectivity. Mao Yanjun and others invented a "process method for extracting lithium from lithium mother liquor and its application, application number: CN202410181886.8". This method uses a microfiltration purification system to remove impurities in the brine, and then uses a nanofiltration salt separation system to nanofilter and separate the diluted brine, and then obtains a lithium-rich concentrate through a membrane concentration system. After deep magnesium removal, a lithium extraction mother liquor is obtained. The removal rate of magnesium sulfate can reach 70-95%, and the recovery rate of lithium can reach 60-80%.
[0005] Another type of mother liquor extraction is based on the Bayer process of alumina production. By adding ion exchange resins, aluminum-based adsorbents, organic-inorganic composite adsorbents, etc. to the Bayer mother liquor, lithium ions are selectively extracted from the solution to prepare lithium carbonate. Zhang Wanyu and others invented a "method for extracting lithium from the circulating mother liquor of alumina produced by the Bayer process to prepare battery-grade lithium carbonate, classification number: CN202211440254.6". The extraction agent is fully contacted with the circulating mother liquor of alumina produced by the Bayer process, and the organic phase of lithium is separated by washing with strong acid, and then lithium precipitation, filtration, washing, drying and crushing are performed to obtain battery-grade lithium carbonate. It has the characteristics of short process flow, low cost, high recovery rate and wide application field. Li Yongchun and others used aluminum electrolyte as raw material and invented "a method for extracting lithium from aluminum electrolyte to prepare lithium carbonate, application number: CN202311445085.X". The lithium aluminum electrolyte and organosiloxane were roasted at 200-800 ° C to generate an oxidized mixture containing aluminum, sodium, lithium and potassium. The metal composite oxide was then desiliconized, aluminum hydroxide was added as a seed to precipitate lithium, the pH was adjusted, and CO2 was carbonized to obtain crude lithium carbonate. The entire process overcomes the low recovery rate of Li metal leaching in the acid leaching process, reduces the escape of hydrogen fluoride, and the lithium extraction efficiency can reach 90%
[0006] Although the reduction burning, reagent flotation and wet acid leaching technologies can achieve a high lithium extraction rate in the direct extraction process of ore, the main element aluminum in bauxite is not fully utilized, and the production cost is high. On the other hand, the mother liquor extraction process has little impact on the main process of the Bayer process, but the main problem currently faced is how to improve the lithium extraction rate and how to maintain the performance stability of exchange resins, adsorbents, etc. in the Bayer mother liquor. Summary of the invention
[0007] In order to improve the selectivity and adsorption capacity of montmorillonite for lithium ions in Bayer circulating mother liquor, the present invention provides a preparation method of intercalated crown ether montmorillonite for selective adsorption of lithium. Montmorillonite has a unique 2:1 unit structure layer and a large layer charge (0.2<e<6), and has excellent cation exchange capacity (70~130 mmol / 100g). Through isomorphous substitution in the crystal structure, Li + , K + , Ca 2+Ions enter the structural layer in the form of hydrated cations. Montmorillonite has excellent ion exchange performance, but its ion exchange process is not highly selective, and there are problems of interference from impurity ions such as sodium, potassium, aluminum, and calcium. 12-crown ether-4, which is selective for lithium ions, is embedded in the layered structure of montmorillonite, and the O in the epoxy group of 12-crown ether-4 coordinates with the Li ions to form Li-O. The four O atoms in the epoxy group are used as electron donors. After coordination, two O atoms protrude from the plane and form a tetrahedral structure with the Li ions, achieving specific capture of Li ions, thereby achieving efficient and selective adsorption of lithium ions in Bayer mother liquor. The technical solution of the present invention is implemented according to the following steps:
[0008] (1) Weigh calcium montmorillonite and place it in a 65°C constant temperature drying oven for 12-24 h. Grind and sieve it. The average particle size of the calcium montmorillonite is 70 μm and the specific surface area is 50 m 2 / g, and the cation exchange capacity (CEC) of montmorillonite was 0.96 mmol / g as measured by the ammonium chloride-ethanol method;
[0009]
[0010] (2) Add the treated montmorillonite and deionized water into a magnetic stirrer and stir for 3-6 h. The stirring temperature of the magnetic stirrer is 40 °C and the stirring speed is 300 r / min. After stirring evenly, a montmorillonite suspension A1 is obtained. The liquid-to-solid ratio of the montmorillonite suspension A1 is 100 ml / g.
[0011] (3) The montmorillonite suspension A1 was placed in an ultrasonic dispersion device for 10 min at an ultrasonic power of 600 W to obtain a montmorillonite dispersion solution A2;
[0012] (4) The weighed 12-crown ether-4 is added to the montmorillonite dispersion solution A2, and the molar ratio of montmorillonite to the added 12-crown ether-4 in solution A2 is 10:1-20:1. Solution A2 is placed in a rotary mixer and mixed in the rotary mixer for 4 hours. Crown ether molecules have a certain macrocyclic structure. Based on the macrocyclic effect (superchelation effect), when metal cations and crown ethers form a complex, they have relatively stable properties. At the same time, the macrocyclic ligands of crown ethers have an adjustable cavity structure. If the size of the metal ion matches the cavity diameter of the crown ether, a stable complex can be formed, thereby obtaining excellent selectivity for the coordinated metal ions. The cavity diameter of 12-crown ether-4 is similar to the metal radius of lithium ions. It is embedded in the layered structure of montmorillonite. On the basis of retaining the specific vacancies of the epoxy group of 12-crown ether-4, it is stably present in the montmorillonite structure layer, and a solution A3 containing montmorillonite embedded with 12-crown ether-4 is obtained;
[0013] (5) Place solution A3 in a centrifuge and centrifuge at 3000 r / min for 10 min, wash repeatedly with high-purity water 4-5 times, and let stand to obtain a solid sample B1;
[0014] (6) Sample B1 was placed in a freeze dryer and freeze-dried for 12 h. The dried sample was ground and sieved to obtain a modified montmorillonite embedded with 12-crown ether-4.
[0015] (7) The modified montmorillonite embedded with 12-crown ether-4 was added as an adsorbent to the sodium aluminate solution A4 with a molecular ratio of 1.5. The O in the epoxy group of 12-crown ether-4 coordinated with the lithium ions in the sodium aluminate solution to form Li-O. The four O atoms in the epoxy group acted as electron donors. After coordination, two O atoms protruded from the plane and formed a tetrahedral structure with the lithium ions to selectively adsorb lithium ions. The adsorption time was 60 min, the solution temperature was 80 °C, and the liquid-solid ratio of montmorillonite and ammonium aluminate solution A4 was 200-400 ml / g.
[0016] The advantages of the present invention are: (1) the structure of the crown ether montmorillonite in the mother liquor before seeding is stable, and the Li ion adsorption efficiency is high and the selectivity is good; (2) the desorption efficiency of citric acid on the lithium-rich montmorillonite is high, the montmorillonite can be recycled after desorption, and the desorption liquid (lithium citrate) can be directly used for the preparation of lithium battery positive electrode materials; (3) the process will not introduce impurities, the ion selectivity is good, and it has no effect on the Bayer process system. The new idea realizes the efficient recovery of lithium in the mother liquor without changing the original alumina production process, which has important guiding significance for the effective utilization of lithium resources in lithium-containing bauxite. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION
[0018] The present invention is further described in detail below in conjunction with the embodiments.
[0019] Implementation Example 1
[0020] The particle size of calcium-based montmorillonite raw material is 50 μm and the specific surface area is 40 m 2 / g, and the cation exchange capacity (CEC) is 1.24mmol / g.
[0021] (1) Weigh 10 g of calcium montmorillonite and place it in a 65 °C constant temperature drying oven. Dry it for 12-24 h, then grind it and pass it through a 200 mesh sieve.
[0022] (2) Add the dried montmorillonite and 1000 ml of deionized water into a magnetic stirrer and stir for 2 h. The liquid-to-solid ratio of montmorillonite to deionized water is 100 ml / g. The stirring temperature is 40 °C and the stirring speed is 300 r / min to obtain a montmorillonite suspension.
[0023] (3) placing the montmorillonite suspension in an ultrasonic dispersion device for 20 min at an ultrasonic power of 500 W to obtain a montmorillonite dispersion;
[0024] (4) Weigh 0.2 g of 12-crown-4 and montmorillonite dispersion solution and add them into a rotary mixer, the molar ratio of montmorillonite 12-crown-4 to montmorillonite being 15:1. The mixing time in the rotary mixer is 4 h. Then, the mixed solution is taken out and centrifuged in a centrifuge for 30 min at a centrifugal speed of 4500 r / min.
[0025] (5) Repeat the above centrifugation step 5 times, freeze-dry the precipitated solid for 12 h, grind and sieve to obtain montmorillonite embedded with 12-crown ether-4;
[0026] (6) A sodium aluminate solution with a molecular weight ratio of 1.6 was prepared, and the prepared 12-crown ether-4 montmorillonite was used as an adsorbent to selectively adsorb lithium ions from the sodium aluminate solution. The liquid-to-solid ratio of montmorillonite and sodium aluminate solution was 250 ml / g, the temperature of the sodium aluminate solution was 70 °C, the adsorption time was 120 min, and the final lithium removal rate was 76%.
[0027] Implementation Example 2
[0028] The particle size of calcium-based montmorillonite raw material is 70 μm and the specific surface area is 60 m 2 / g, and the cation exchange capacity (CEC) is 0.98mmol / g.
[0029] (1) Weigh 10 g of calcium montmorillonite and place it in a 65 °C constant temperature drying oven. Dry it for 12 h, then grind it and pass it through a 200 mesh sieve.
[0030] (2) Add the dried montmorillonite and 2000 ml of deionized water into a magnetic stirrer and stir for 4 h. The liquid-to-solid ratio of montmorillonite to deionized water is 200 ml / g. The stirring temperature is 40 °C and the stirring speed is 300 r / min to obtain a montmorillonite suspension.
[0031] (3) The montmorillonite suspension was placed in an ultrasonic dispersion device for 10 min at an ultrasonic power of 500 W to obtain a montmorillonite dispersion;
[0032] (4) Weigh 0.15 g of 12-crown ether-4 and montmorillonite dispersion solution and add them into a rotary mixer. The molar ratio of montmorillonite 12-crown ether-4 to montmorillonite is 25:1. The mixing time in the rotary mixer is 6 h. Then, the mixed solution is taken out and placed in a centrifuge for centrifugation for 30 min at a centrifugal speed of 4500 r / min.
[0033] (5) Repeat the above centrifugation step 5 times, freeze-dry the precipitated solid for 12 h, grind and sieve to obtain montmorillonite embedded with 12-crown ether-4.
[0034] (6) A sodium aluminate solution with a molecular weight ratio of 1.5 was prepared, and the prepared 12-crown ether-4 montmorillonite was used as an adsorbent to selectively adsorb lithium ions from the sodium aluminate solution. The liquid-to-solid ratio of montmorillonite and sodium aluminate solution was 400 ml / g, the temperature of the sodium aluminate solution was 80 °C, the adsorption time was 120 min, and the final lithium removal rate was 83%.
Claims
1. A method for preparing a crown ether montmorillonite for selectively adsorbing lithium, involving the intercalation modification of montmorillonite, comprising the following steps: (1) Place the calcium-based montmorillonite in a 65°C constant temperature drying oven and dry it for 12-24 hours, then grind and sieve it; (2) Add the treated natural calcium-based montmorillonite and deionized water into a magnetic stirrer and stir for 3-6 h to obtain a montmorillonite suspension A1; (3) placing the montmorillonite suspension A1 into an ultrasonic dispersion device, and obtaining a solution A2 after ultrasonic dispersion; (4) adding 12-crown ether-4 to solution A2 and mixing in a rotary mixer for 4 h, so that the 12-crown ether-4 epoxy group is stably present in the montmorillonite structure layer while retaining the specific vacancies of the 12-crown ether-4 epoxy group, thereby obtaining a mixed solution A3 containing montmorillonite embedded with 12-crown ether-4; (5) Place solution A3 in a centrifuge and centrifuge for 10 min. Repeat the washing of the lower solid layer with high-purity water for 4-5 times. After standing for 30 min, obtain sample B1. (6) Sample B1 was placed in a freeze dryer for freeze drying for 12 h, and then ground and sieved to obtain modified montmorillonite embedded with 12-crown ether-4; (7) The modified montmorillonite embedded with 12-crown ether-4 was added to the sodium aluminate solution A4 as an adsorbent to selectively adsorb lithium in the solution for 60 min.
2. The method for preparing a crown ether montmorillonite for selectively adsorbing lithium according to claim 1, characterized in that The average particle size of the calcium-based montmorillonite in step (1) is 70 μm, and the specific surface area is 50 m 2 / g, and the cation exchange capacity (CEC) is 0.96 mmol / g.
3. The method for preparing a crown ether montmorillonite for selectively adsorbing lithium according to claim 1, characterized in that In the step (2), the stirring temperature of the magnetic stirrer is 40°C, the stirring speed is 300 r / min, and the liquid-to-solid ratio of the montmorillonite suspension A1 is 100 ml / g.
4. The method for preparing a crown ether montmorillonite for selectively adsorbing lithium according to claim 1, characterized in that The ultrasonic power in step (3) is 600 W and the ultrasonic time is 10 min.
5. The method for preparing a crown ether montmorillonite for selectively adsorbing lithium according to claim 1, characterized in that In the step (4), the molar ratio of montmorillonite to 12-crown ether-4 added to the solution is 10:1-20:
1.
6. The method for preparing a crown ether montmorillonite for selectively adsorbing lithium according to claim 1, characterized in that The centrifuge speed in step (5) is 3000 r / min.
7. The method for preparing a crown ether montmorillonite for selectively adsorbing lithium according to claim 1, characterized in that The O in the 12-crown-4-epoxy group added in step (7) coordinates with the Li ion to form Li-O, and the four O atoms in the epoxy group serve as electron donors. After coordination, two O atoms protrude from the plane and form a tetrahedral structure with the Li ion, thereby achieving selective adsorption of lithium ions; The molecular ratio of A4 solution is 1.5, the solution temperature is 80 °C, the liquid-solid ratio of modified montmorillonite and A3 is 200-400 ml / g, and the removal rate of lithium in the final solution can reach 60-80%.
Citation Information
Patent Citations
Preparation method of modified nano montmorillonite
CN113247917A
Method for extracting scattered element lithium from Bayer process sodium aluminate solution
CN116240401A
Lithium ion specific adsorbent and preparation method and application thereof
CN118079872A