Preparation method of MOF-based silver monatomic adsorption material and application of MOF-based silver monatomic adsorption material in low-concentration bromide ion adsorption
Through the preparation of MOF-based silver single-atom adsorption material, N-anchored silver is used to improve the adsorption efficiency of bromide ions, solving the problems of low-concentration bromide ions and low utilization rate of precious metals in the prior art, and achieving high-efficiency bromide Ion adsorption and efficient utilization of silver.
Patent Information
- Application Number
- CN202411480196.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-23
- Publication Date
- 2024-11-22
AI Technical Summary
The existing adsorption materials have small adsorption capacity in low concentration bromide ion adsorption, and the utilization rate of precious metal atoms is not high, resulting in low extraction efficiency and high cost.
Using MOF-based silver single atom adsorption material, the monodispersion of silver is achieved by anchoring silver by N, which improves the adsorption rate of bromide ions and the utilization rate of silver. The preparation method includes thermal reaction between zirconium salt and organic ligand and silver salt. Post-treatment to form an efficient bromide adsorbent.
The adsorption capacity and adsorption efficiency of low-concentration bromide ions are significantly improved. The adsorption capacity of silver reaches 2012 mg/gAg, which can achieve 100% adsorption within 10 minutes, and the process is simple and suitable for industrial production.
Smart Images

Figure CN118988267A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of adsorption materials, and in particular relates to a preparation method of a MOF-based silver single-atom adsorption material and application thereof in low-concentration bromide ion adsorption. Background Art
[0002] Bromine, known as the "marine element", is an important basic chemical raw material and the mainstay of the marine chemical industry. A wide variety of inorganic bromides, bromates and bromine-containing organic compounds derived from bromine have special value in the national economy and scientific and technological development. With the development of my country's leading industries, they are penetrating into various industries and fields, and are mainly used in: pesticides, dyes, brominated flame retardants and refrigerants. Bromine mainly comes from liquid ores, including seawater, salt lakes and oilfield water. The bromine extraction methods commonly used internationally can be roughly divided into: air blowing method, steam distillation method, solvent extraction method, ion exchange resin method, adsorbent method, membrane separation method, etc. These methods have various disadvantages, such as large investment, high energy consumption, immature technology, or cannot be applied to solutions with low bromine content. However, the adsorption method is very effective in directly extracting low-concentration Br − This method shows great potential in extracting low-concentration bromide ions more safely and energy-efficiently. In recent years, a series of metal-organic frameworks (MOFs) have become very promising adsorption materials due to their water stability, high tunability and porosity. At the same time, due to their large specific surface area, they are often used as carriers of precious metal Ag nanoparticles to synergistically adsorb bromide ions. However, due to the very limited atomic utilization of silver nanoparticles, the precious metal is wasted. Summary of the invention
[0003] In view of the shortcomings of the current adsorption materials, such as small adsorption capacity and low utilization rate of precious metal atoms, the present invention provides a method for preparing a MOF-based silver single-atom adsorption material and its application in low-concentration bromide ion adsorption. Compared with traditional silver-based adsorbents, the adsorption capacity of the MOF-based silver single-atom adsorption material of the present invention is improved, and the atomic utilization rate of precious metal silver is greatly improved, and it is a highly efficient bromide ion adsorbent.
[0004] The present invention utilizes N-anchored silver on the MOF ligand to achieve monodispersity of silver, and compared with silver nanoparticles loaded on other MOFs, the adsorption rate of bromide ions and the utilization rate of silver are improved.
[0005] The preparation method of the MOF-based silver single atom adsorption material of the present invention comprises the following steps: Step 1: Take a certain amount of zirconium salt and organic ligand and add them to a solvent, transfer the mixture to a reactor and heat it for reaction, wash and dry it after the reaction is completed to obtain UiO-bpy.
[0006] Step 2: Dissolve the obtained UiO-bpy and silver salt in a solvent, stir and react for a period of time, separate and collect the solid, wash and dry it to obtain a MOF-based silver single atom adsorption material.
[0007] in: In step 1, the zirconium salt is zirconium chloride.
[0008] In step 1, the organic ligand is 2,2'-bipyridine-5,5'-dicarboxylic acid.
[0009] Furthermore, the molar ratio of the zirconium salt to the organic ligand is 1:1.
[0010] In step 1, the solvent is DMF.
[0011] In step 1, the heating reaction temperature is 120° C. and the reaction time is 24 h.
[0012] In step 2, the silver salt is silver nitrate.
[0013] In step 2, the solvent is tetrahydrofuran. The mass ratio of the silver salt to the UiO-bpy is 0.5:1 to 2:1, preferably 1:1.
[0014] In step 2, the reaction temperature is room temperature, the reaction time is 12 hours, and the drying condition is 60° C. for 12 hours.
[0015] The MOF-based silver single atom adsorption material prepared by the present invention is used in the adsorption of low-concentration bromide ions.
[0016] The low concentration refers to a bromide ion concentration of ≤100 ppm.
[0017] Weigh a certain amount of MOF-based silver single-atom adsorption material and add it to 100 mL of a solution containing bromide ions. Place the solution in a constant temperature oscillator and perform oscillation adsorption under constant temperature conditions. Measure and analyze the remaining bromide ion concentration in the aqueous solution at regular intervals until equilibrium is reached. The adsorption capacity Qe is calculated using the following formula:
[0018] Where: Qe is the saturated adsorption capacity of MOF-based silver atoms at equilibrium (mg·g -1 ); Co and Ce are the initial concentrations of bromide ions in the aqueous solution (mg·L -1 ) and the concentration after adsorption equilibrium (mg·L -1 ); m is the mass of the added adsorbent (g); V is the volume of the solution (L).
[0019] The beneficial effects of the present invention are embodied in: 1. The organic ligand-anchored silver atoms in the MOF structure have a strong affinity with bromide ions, and there is a strong chemical reaction between silver and bromide ions, which makes the material have a large adsorption capacity for low-concentration bromide ions in aqueous solution (256 mg / g), and the adsorption capacity of silver can reach 2012 mg / g Ag , which is superior to other silver-based adsorbents reported so far.
[0020] 2. The adsorption rate of the adsorbent material of the present invention for low-concentration bromide ions can reach 100%, and the adsorption can be quickly achieved within 10 minutes. The adsorption rate and adsorption efficiency are both excellent.
[0021] 3. The preparation process of the adsorbent material of the present invention is relatively simple, and it is expected to realize batch preparation and industrial large-scale production of adsorbents. The material provides a highly efficient and significant method for the adsorption of low-concentration bromide ions in water. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.
[0023] Figure 1 is the SEM image of Ag / UiO-bpy. Figure 1 It can be seen that Ag / UiO-bpy has an octahedral morphology.
[0024] Figure 2 This is the TEM image of Ag / UiO-bpy. Figure 2 It can be seen that Ag / UiO-bpy presents an octahedral morphology and there is no agglomeration of silver nanoparticles.
[0025] Figure 3 is the XRD pattern of Ag / UiO-bpy. Figure 3 It can be seen that the crystal structure of UiO-bpy was synthesized without the characteristic peak of silver.
[0026] Figure 4 This is the XRD pattern of Ag / UiO-bpy after adsorption. Figure 4 It can be seen that after adsorption, the main characteristic peak is that of AgBr, and the adsorption of bromide ions is achieved by generating AgBr.
[0027] Figure 5 This is the curve of the adsorption rate of low concentration bromide ions on Ag / UiO-bpy over time. Figure 5It can be seen that the adsorption rate of the adsorbent material of the present invention for low concentration bromide ions can reach 100%, and the adsorption can be quickly achieved within 10 minutes, and the adsorption rate and adsorption efficiency are both excellent.
[0028] Figure 6 It is a bar graph showing the changes in the adsorption rate of bromide ions by Ag / UiO-bpy with different contents under the influence of other competing ions. Figure 6 It can be seen that the adsorption selectivity of the adsorbent material for bromide ions is good. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with examples. The specific examples described here are only used to explain the present invention and do not limit the present invention. Embodiment 1:
[0030] In this embodiment, the MOF-based silver single atom is composed of an organic framework UiO-bpy and single-atom silver, and the preparation method is as follows: 1. Dissolve 0.52 mmol of ZrCl4 and 0.53 mmol of 2,2'-bipyridine-5,5'-dicarboxylic acid in 50 ml of DMF, add 5 mL of formic acid solution, and ultrasonicate at room temperature for 30 min to obtain a white mixed solution. Transfer the mixture to a 100 mL polytetrafluoroethylene-lined autoclave, seal the autoclave and heat it in an oven at 120°C for 24 h. After the autoclave is naturally cooled to room temperature, wash it with DMF solvent three times, and finally put UiO-bpy into a vacuum oven at 60°C and dry it overnight.
[0031] 2. Take 50 mg of UiO-bpy obtained by drying in step 1 and disperse it in 20 mL of THF. Then take 50 mg of AgNO3 and dissolve it in 20 mL of THF and 1 mL of deionized water. Ultrasonicate the two solutions and stir the obtained suspension overnight. In order to prevent the decomposition of silver nitrate by light, wrap tin foil outside the glass bottle. After the reaction, wash it with THF several times and then dry it in a vacuum oven at 60 ° C for 12 h to obtain Ag / UiO-bpy.
[0032] 5 mg of Ag / UiO-bpy prepared in this example was added to 100 ml of 100 ppm potassium bromide solution, the adsorption temperature was 30 ° C, the adsorption time was 10 min, the adsorption rate was 100%, the adsorption capacity was 256 mg / g, and the adsorption capacity of silver could reach 2012 mg / g Ag . Embodiment 2:
[0033] In this embodiment, the MOF-based silver single atom is composed of an organic framework UiO-bpy and single-atom silver, and the preparation method is as follows: 1. Dissolve 0.52 mmol of ZrCl4 and 0.53 mmol of 2,2'-bipyridine-5,5'-dicarboxylic acid in 50 ml of DMF, add 5 mL of formic acid solution, and ultrasonicate at room temperature for 30 min to obtain a white mixed solution. Transfer the mixture to a 100 mL polytetrafluoroethylene-lined autoclave, seal the autoclave and heat it in an oven at 120 °C for 24 h. After the autoclave is naturally cooled to room temperature, wash it with DMF solvent three times, and finally put UiO-bpy into a vacuum oven at 60 °C and dry it overnight.
[0034] 2. Take 50 mg of UiO-bpy obtained by drying in step 1 and disperse it in 20 mL of THF. Then take 100 mg of AgNO3 and dissolve it in 20 mL of THF and 1 mL of deionized water. Ultrasonicate the two solutions and stir the obtained suspension overnight. In order to prevent the decomposition of silver nitrate by light, wrap tin foil outside the glass bottle. After the reaction, wash it with THF several times, and then dry it in a vacuum oven at 60°C for 12 h to obtain Ag / UiO-bpy.
[0035] 5 mg of Ag / UiO-bpy prepared in this example was added to a potassium bromide solution with a concentration of 100 ppm. The adsorption temperature was 30 °C, the adsorption time was 12 h, the adsorption rate was 89.2%, the adsorption capacity was 248 mg / g, and the adsorption capacity of silver could reach 1872 mg / g. Ag . Embodiment 3:
[0036] In this embodiment, the MOF-based silver single atom is composed of an organic framework UiO-bpy and single-atom silver, and the preparation method is as follows: 1. Dissolve 0.52 mmol of ZrCl4 and 0.53 mmol of 2,2'-bipyridine-5,5'-dicarboxylic acid in 50 ml of DMF, add 5 mL of formic acid solution, and ultrasonicate at room temperature for 30 min to obtain a white mixed solution. Transfer the mixture to a 100 mL polytetrafluoroethylene-lined autoclave, seal the autoclave and heat it in an oven at 120 °C for 24 h. After the autoclave is naturally cooled to room temperature, wash it with DMF solvent three times, and finally put UiO-bpy into a vacuum oven at 60 °C and dry it overnight.
[0037] 2. Take 50 mg of UiO-bpy obtained by drying in step 1 and disperse it in 20 mL of THF. Then take 25 mg of AgNO3 and dissolve it in 20 mL of THF and 1 mL of deionized water. Ultrasonicate the two solutions and stir the obtained suspension overnight. In order to prevent the decomposition of silver nitrate by light, wrap tin foil outside the glass bottle. After the reaction, wash it with THF several times and then dry it in a vacuum oven at 60°C for 12 h to obtain Ag / UiO-bpy.
[0038] 5 mg of Ag / UiO-bpy prepared in this example was added to a potassium bromide solution with a concentration of 100 ppm. The adsorption temperature was 30°C, the adsorption time was 12 h, the adsorption rate was 75.5%, the adsorption capacity was 210 mg / g, and the adsorption capacity of silver could reach 1751 mg / g. Ag . Embodiment 4:
[0039] In this embodiment, the MOF-based silver single atom is composed of an organic framework UiO-bpy and single-atom silver, and the preparation method is as follows: 1. Dissolve 0.52 mmol of ZrCl4 and 0.53 mmol of 2,2'-bipyridine-5,5'-dicarboxylic acid in 50 ml of DMF, add 5 mL of formic acid solution, and ultrasonicate at room temperature for 30 min to obtain a white mixed solution. Transfer the mixture to a 100 mL polytetrafluoroethylene-lined autoclave, seal the autoclave and heat it in an oven at 120 °C for 24 h. After the autoclave is naturally cooled to room temperature, wash it with DMF solvent three times, and finally put UiO-bpy into a vacuum oven at 60 °C and dry it overnight.
[0040] 2. Take 50 mg of UiO-bpy obtained by drying in step 1 and disperse it in 20 mL of THF. Then take 10 mg of AgNO3 and dissolve it in 20 mL of THF and 1 mL of deionized water. Ultrasonicate the two solutions and stir the obtained suspension overnight. In order to prevent the decomposition of silver nitrate by light, wrap tin foil outside the glass bottle. After the reaction, wash it with THF several times, and then dry it in a vacuum oven at 60°C for 12 h to obtain Ag / UiO-bpy.
[0041] 5 mg of Ag / UiO-bpy prepared in this example was added to a potassium bromide solution with a concentration of 100 ppm. The adsorption temperature was 30°C, the adsorption time was 12 h, the adsorption rate was 46.6%, the adsorption capacity was 126 mg / g, and the adsorption capacity of silver could reach 1348 mg / g. Ag . Embodiment 5:
[0042] 15 mg of Ag / UiO-bpy prepared in Example 1 was added to 100 ml of a mixed solution with a bromide ion and a nitrate ion concentration of 100 ppm. The adsorption temperature was 30 ° C, the adsorption time was 12 h, the adsorption rate was 92.13%, the adsorption capacity was 86 mg / g, and the adsorption capacity of silver could reach 967 mg / g. Ag The adsorbent has the selective adsorption to bromide ions in the presence of nitrate ions. Embodiment 6:
[0043] 15 mg of Ag / UiO-bpy prepared in Example 1 was added to 100 ml of a mixed solution with a bromide ion concentration of 100 ppm and a chloride ion concentration of 0.5 M. The adsorption temperature was 30 ° C, the adsorption time was 12 h, the adsorption rate was 54.8%, the adsorption capacity was 73 mg / g, and the adsorption capacity of silver could reach 852 mg / g. Ag The adsorbent still has a certain adsorption selectivity for bromide ions in the presence of high concentrations of chloride ions, and can be effectively used to adsorb bromide ions in actual seawater environments. Embodiment 7:
[0044] The adsorbed Ag / UiO-bpy in Example 1 was washed three times with deionized water by centrifugation, and then dried in a vacuum oven at 60°C for 12 h. 20 mg of the dried powder was added to 100 ml of a solution with an iodine ion concentration of 200 ppm. The solution was exposed to sunlight for 8 h on a sunny day at a temperature of about 25°C. The concentration of bromide ions in the solution after the reaction was measured, and the desorption rate was calculated. The desorption rate was 78.8%. The adsorbent had excellent adsorption and desorption effects on bromide ions, and could effectively extract bromide ions.
Claims
1. A method for preparing a MOF-based silver single atom adsorption material, characterized in that The steps include: Step 1: Take a certain amount of zirconium salt and organic ligand and add them to the solvent, transfer the mixture to a reactor and heat it for reaction, wash and dry it after the reaction is completed to obtain UiO-bpy; Step 2: Dissolve the obtained UiO-bpy and silver salt in a solvent, stir and react for a period of time, separate and collect the solid, wash and dry it to obtain a MOF-based silver single atom adsorption material.
2. The preparation method according to claim 1, characterized in that: In step 1, the zirconium salt is zirconium chloride, and the organic ligand is 2,2'-bipyridine-5,5'-dicarboxylic acid.
3. The preparation method according to claim 2, characterized in that: The molar ratio of the zirconium salt to the organic ligand is 1:
1.
4. The preparation method according to claim 1, characterized in that: In step 1, the heating reaction temperature is 120° C. and the reaction time is 24 h.
5. The preparation method according to claim 1, characterized in that: In step 2, the silver salt is silver nitrate.
6. The preparation method according to claim 1, characterized in that: In step 2, the mass ratio of the silver salt to the UiO-bpy is 0.5:1-2:
1.
7. The preparation method according to claim 6, characterized in that: The mass ratio of the silver salt to the UiO-bpy is 1:
1.
8. The preparation method according to claim 1, characterized in that: In step 2, the reaction temperature is room temperature and the reaction time is 12 h.
9. Use of the MOF-based silver single atom adsorption material prepared by the preparation method according to any one of claims 1 to 8 in the adsorption of low-concentration bromide ions.
10. The use according to claim 9, characterized in that: The low concentration refers to a bromide ion concentration of ≤100 ppm.
Citation Information
Cited By
Silver ion functionalized covalent organic framework material as well as preparation method and application thereof
CN119708402A