UiO-66-derived Ru / ZrO2 catalyst and application of preparation method of UiO-66-derived Ru / ZrO2 catalyst in preparation of methane by photothermal catalysis of carbon dioxide hydrogenation
Ru particles were grown in situ by UiO-66-derived ZrO2 support, and combined with photothermal effect, a high-activity and good selectivity Ru/ZrO2 catalyst was prepared, which solved the problem of insufficient catalyst activity in the prior art and achieved efficient carbon dioxide addition The effect of converting hydrogen into methane.
Patent Information
- Application Number
- CN202411074172.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
In the catalytic conversion of carbon dioxide hydrogenation, the activity and selectivity of the catalyst are insufficient, and there is a lack of research on oxide catalysts derived from MOF support materials, resulting in low catalytic efficiency.
Using ZrO2 derived from UiO-66 as a support, metal particles Ru are grown in situ, and an octahedral Ru/ZrO2 catalyst is prepared. Combined with the photothermal effect, the specific surface area and active sites of the catalyst are increased, the energy barrier of the thermal catalytic reaction is reduced, and the catalytic activity is enhanced. .
It has achieved high activity, selectivity and stability of photothermal CO2 hydrogenation to methane catalyst, with excellent catalytic performance and is suitable for industrial applications.
Smart Images

Figure CN118988296A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of carbon dioxide hydrogenation catalytic conversion, and in particular to a metal particle Ru-loaded ZrO2 catalyst for carbon dioxide hydrogenation catalytic synthesis of methane, and a preparation method and application thereof. Background Art
[0002] The environmental impact of excessive carbon dioxide emissions is rapidly increasing, so in order to achieve net carbon emissions and reduce dependence on fossil fuels, the efficient conversion of carbon dioxide into value-added fuels using renewable energy has been widely studied. Among various carbon dioxide (CO2) conversion methods, CO2 is hydromethanated to produce artificial CH4, which has attracted great interest from the research and industrial communities because CH4 can be further used as a chemical feedstock to produce high-value-added chemical products and as an efficient medium to store energy in high-energy bonds for storage and transportation.
[0003] Photothermal catalytic carbon dioxide reduction combines photocatalysis and traditional thermal catalysis, and has become a new and expanding research direction in recent years. Photothermal catalysis is a catalytic reaction driven by the photothermal effect (a combination of photochemistry and thermochemistry of sunlight), which exists in various catalytic materials (semiconductors, plasma metals, composite catalysts). When light irradiates a semiconductor, the incident photons excite the semiconductor with an energy equal to or greater than the band gap, generating electrons and holes; some electrons and holes then move to the catalyst surface to participate in the redox process. In semiconductors, the photothermal effect is based on the generation of photogenerated carriers, a portion of the electron-hole pairs dissipate the input energy in the form of radiation (emitted photons) or non-radiation (excited phonons), and heat can be generated through lattice vibrations during non-radiation. The photothermal conversion efficiency of the catalyst is closely related to the band gap width of the semiconductor, and narrow band gap semiconductors are more efficient in converting light energy into thermal energy. Plasmonic metals (Ni, Ag, etc.) cause local heating due to the local surface plasmon resonance effect, providing heat and hot electrons to promote the CO2 reduction reaction. At present, many scholars have devoted themselves to the study of Ru and its composite catalysts. For example, Ge et al. studied Ru / H x MoO 3-y The catalyst plasma effect promotes the photothermal catalytic CO2 methanation, and 20.8 mmol·g was achieved in CO2 methanation under Vis-NIR light irradiation at 140 °C. cat -1 ·h -1 (520mmol·g Ru -1 ·h -1) CH4 yield and 100% selectivity. S Tada studied Ru / CeO2 / Al2O3 catalysts to improve the selectivity of CO2 methanation CH4 at low temperature. Wang Ke et al. studied Ru / TiO2 photothermal catalysts using Ru-rich surface oxygen vacancies and photogenerated electrons-holes generated by TiO2 carriers to improve their CO2 methanation activator efficiency. Hironori Nagase studied the effects of carrier materials and preparation methods on the CO2 methanation activity of Ru nanoparticles in the crystalline and amorphous states of the carrier in Ru / ZrO2. However, there are few studies on oxide catalysts derived from MOF carrier materials. MOF carriers generally have a larger specific surface area and a smaller void structure and often have better catalytic performance. Therefore, it is necessary to synthesize nanostructured ZrO2 (such as ZrO2 nanohexahedrons, ZrO2 octahedrons, CeO2 dodecahedrons, etc.) with different morphologies under different conditions as catalysts or catalytic carriers. The derived oxides also have different surface structures and active sites, which have different effects on catalysis. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a UiO-66-derived Ru / ZrO2 catalyst and a preparation method and application thereof. The present invention increases the specific surface area and effective active sites of the material by morphology control of Zr-MOF (UiO-66), effectively improving the effective catalytic specific surface area of the catalyst. At the same time, Ru-loaded UiO-66 is derived into octahedral Ru / ZrO2 to promote photogenerated charge transfer under illumination conditions and reduce the energy barrier of thermal catalytic reaction to improve the catalytic activity of the catalyst, thereby obtaining a photothermal CO2 hydrogenation to methane catalyst material with high activity, selectivity, stability and safety.
[0005] In order to solve the existing technology, the technical solution adopted by the present invention is:
[0006] On one hand, the present invention discloses a Ru / ZrO2 catalyst derived from UiO-66. The Ru / ZrO2 catalyst is obtained by in-situ growing metal particles Ru on the surface of octahedral ZrO2 derived from UiO-66 and calcining the resulting catalyst.
[0007] Furthermore, the preparation method of the Ru / ZrO2 catalyst comprises the following steps:
[0008] Step 1: dissolving ZrCl4 in DMF and stirring evenly to obtain a ZrCl4 DMF solution; dissolving terephthalic acid in the DMF solution at room temperature, and then mixing with the ZrCl4 DMF solution, and continuing to stir, slowly adding acetic acid dropwise during the stirring process, and after the stirring is completed, transferring the mixed solution to a stainless steel autoclave lined with polytetrafluoroethylene for hydrothermal reaction, and after the reaction is completed, cooling the autoclave to room temperature, taking out and centrifuging to collect the white precipitate, washing, drying, and grinding to obtain white UiO-66 powder;
[0009] Step 2: Place the white UiO-66 powder and PVP in a conical flask filled with deionized water and sonicate to obtain a uniform dispersion;
[0010] Step 3: Dissolve RuCl3·xH2O in the dispersion, stir magnetically, add ammonia water dropwise during stirring until the pH is 10, continue heating and stirring in a water bath after stirring, wait until it cools to room temperature, centrifuge, wash, and dry to obtain a MOF precursor of Ru / UiO-66;
[0011] Step 4: Place the MOF precursor of Ru / UiO-66 in a covered quartz crucible in a muffle furnace, calcine, and grind after cooling to obtain a dark green Ru / ZrO2 catalyst.
[0012] Furthermore, in step 1, the molar ratio of ZrCl4 to terephthalic acid is 1:1; and the volume ratio of DMF to acetic acid is 6:1.
[0013] Furthermore, in step 1, the hydrothermal reaction temperature is 120° C. and the reaction time is 24 h.
[0014] Furthermore, in step 2, the mass ratio of UiO-66 powder to PVP is 3:1.
[0015] Furthermore, in step 3, the mass ratio of RuCl3·xH2O and UiO-66 powder is 0.01-0.09:1.
[0016] Furthermore, in step 3, the water bath heating stirring temperature is 60° C., and the stirring time is 3 h.
[0017] Furthermore, in step 4, the calcination temperature is 500° C., a temperature program is set, and the rate of the temperature program is 5° C. / min. After the temperature reaches 500° C., the temperature is kept constant for 2 hours.
[0018] On the other hand, the present invention also discloses the use of Ru / ZrO2 catalyst derived from UiO-66 in the preparation of methane by hydrogenation of carbon dioxide, wherein the reaction raw gas used in the application consists of CO2 and H2.
[0019] Furthermore, the flow rate ratio of CO2 and H2 is 1:3-4, the reaction temperature is 170-250°C, and the reaction pressure is 0.5-1.5MPa.
[0020] Furthermore, the flow rate ratio of CO2 and H2 is 1:4, the reaction temperature is 250°C, and the reaction pressure is 1 MPa.
[0021] Beneficial effects of the present invention:
[0022] (1) The present invention uses Zr-MOF as a precursor to synthesize octahedral ZrO2 and in-situ grows Ru on the surface of octahedral ZrO2, successfully preparing Ru / ZrO2 octahedral catalyst. Ru / ZrO2 catalyst has the advantages of large specific surface area and high catalytic activity, and the preparation method is simple, fast and efficient, and has good application prospects.
[0023] (2) The catalyst of the present invention has excellent catalytic performance, and both CO2 conversion rate and methane selectivity are excellent. Compared with catalysts loaded with metal particles in different proportions, the methane yield is the highest when loaded with 7%.
[0024] (3) The catalyst prepared by the present invention through scientific proportions has good catalytic activity under relatively mild reaction conditions, and the preparation method is simple, rapid and efficient, which can provide broad prospects for the subsequent industrial application of methane. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings are used to provide further explanation of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0026] Figure 1 Activity test results of catalysts prepared under different parameters under photothermal and thermal conditions, (a) CO2 conversion rate under thermal catalysis, (b) CO2 conversion rate under photothermal catalysis, (c) space-time yield and selectivity of CH4 under thermal catalysis, (d) space-time yield and selectivity of CH4 under photothermal catalysis;
[0027] Figure 2 XRD test diagrams of catalysts prepared under different parameters;
[0028] Figure 3 These are the SEM and TEM images of the corresponding products in the preparation process of Example 4 of the present invention, where (a) and (b) are the prepared Zr-MOF (UiO-66), (c) is the 7% Ru / ZrO2 prepared in Example 4, and (dg) are the EDS images of Example 4. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the following embodiments.
[0030] Example 1
[0031] A method for preparing a metal particle Ru-loaded ZrO2 catalyst for catalytic synthesis of methane by hydrogenation of carbon dioxide comprises the following steps:
[0032] Step 1: Dissolve 5mM ZrCl4 in 30mL DMF and stir to obtain ZrCl4 DMF solution. Then dissolve 5mM in 30mL DMF and stir to obtain terephthalic acid DMF solution. Subsequently, mix the above two solutions and stir for 30min. Slowly add 10mL of acetic acid during stirring. After stirring, transfer the mixed solution to a stainless steel autoclave lined with polytetrafluoroethylene and hydroheat at 120℃ for 24h. After the reactor cools to room temperature, take out and collect the white precipitate by centrifugation. In a vacuum drying oven at 60℃ for 12h, UiO-66 white powder is obtained.
[0033] Step 2: 0.6 g of UiO-66 white powder and 0.2 g of PVP in step 1 were placed in a conical flask filled with deionized water and ultrasonicated for 15 minutes to obtain a uniform dispersion;
[0034] Step 3: Dissolve 6 mg of RuCl3·xH2O in the dispersion, stir magnetically for 30 min, and then add ammonia water dropwise during stirring until the pH is 10. After stirring, transfer the conical flask containing the mixed solution to a water bath and stir at 60°C for 3 h. After the water bath, cool to room temperature and centrifuge, and wash with deionized water 3 times. Finally, transfer the washed sample to an oven and dry at 80°C for 12 h to obtain the MOF precursor of Ru / UiO-66.
[0035] Step 4: Place the precursor in a covered quartz crucible in a muffle furnace, heat it to a target temperature of 500°C at a rate of 5°C / min and maintain the constant temperature for 2 hours. After cooling, grind to obtain a dark green catalyst, recorded as 1wt% Ru / ZrO2.
[0036] Example 2
[0037] A method for preparing a metal particle Ru-loaded ZrO2 catalyst for catalytic synthesis of methane by hydrogenation of carbon dioxide comprises the following steps:
[0038] Step 1: Dissolve 5mM ZrCl4 in 30mL DMF and stir to obtain ZrCl4 DMF solution. Then dissolve 5mM in 30mL DMF and stir to obtain terephthalic acid DMF solution. Subsequently, mix the above two solutions and stir for 30min. Slowly add 10mL of acetic acid during stirring. After stirring, transfer the mixed solution to a stainless steel autoclave lined with polytetrafluoroethylene and hydroheat at 120℃ for 24h. After the reactor cools to room temperature, take out and collect the white precipitate by centrifugation. In a vacuum drying oven at 60℃ for 12h, UiO-66 white powder is obtained.
[0039] Step 2: 0.6 g of UiO-66 white powder and 0.2 g of PVP in step 1 were placed in a conical flask filled with deionized water and ultrasonicated for 15 minutes to obtain a uniform dispersion;
[0040] Step 3: Dissolve 18 mg of RuCl3·xH2O in the dispersion, stir magnetically for 30 min, and then add ammonia water dropwise during stirring until the pH is 10. After stirring, transfer the conical flask containing the mixed solution to a water bath and stir at 60°C for 3 h. After the water bath, cool to room temperature and centrifuge, and wash with deionized water 3 times. Finally, transfer the washed sample to an oven and dry at 80°C for 12 h to obtain the MOF precursor of Ru / UiO-66.
[0041] Step 4: Place the precursor in a covered quartz crucible in a muffle furnace, heat it to the target temperature of 500°C at a rate of 5°C / min and maintain the constant temperature for 2 hours. After cooling, grind to obtain a dark green catalyst, recorded as 3wt% Ru / ZrO2.
[0042] Example 3
[0043] A method for preparing a metal particle Ru-loaded ZrO2 catalyst for catalytic synthesis of methane by hydrogenation of carbon dioxide comprises the following steps:
[0044] Step 1: Dissolve 5mM ZrCl4 in 30mL DMF and stir to obtain ZrCl4 DMF solution. Then dissolve 5mM in 30mL DMF and stir to obtain terephthalic acid DMF solution. Subsequently, mix the above two solutions and stir for 30min. Slowly add 10mL of acetic acid during stirring. After stirring, transfer the mixed solution to a stainless steel autoclave lined with polytetrafluoroethylene and hydroheat at 120℃ for 24h. After the reactor cools to room temperature, take out and collect the white precipitate by centrifugation. In a vacuum drying oven at 60℃ for 12h, UiO-66 white powder is obtained.
[0045] Step 2: 0.6 g of UiO-66 white powder and 0.2 g of PVP in step 1 were placed in a conical flask filled with deionized water and ultrasonicated for 15 minutes to obtain a uniform dispersion;
[0046] Step 3: Dissolve 30 mg of RuCl3·xH2O in the dispersion, stir magnetically for 30 min, and then add ammonia water dropwise during stirring until the pH is 10. After stirring, transfer the conical flask containing the mixed solution to a water bath and stir at 60°C for 3 h. After the water bath, cool to room temperature and centrifuge, and wash with deionized water 3 times. Finally, transfer the washed sample to an oven and dry at 80°C for 12 h to obtain the MOF precursor of Ru / UiO-66.
[0047] Step 4: Place the precursor in a covered quartz crucible in a muffle furnace, heat it to the target temperature of 500°C at a rate of 5°C / min and maintain the constant temperature for 2 hours. After cooling, grind it to obtain a dark green catalyst, recorded as 5wt% Ru / ZrO2.
[0048] Example 4
[0049] A method for preparing a metal particle Ru-loaded ZrO2 catalyst for catalytic synthesis of methane by hydrogenation of carbon dioxide comprises the following steps:
[0050] Step 1: Dissolve 5mM ZrCl4 in 30mL DMF and stir to obtain ZrCl4 DMF solution. Then dissolve 5mM in 30mL DMF and stir to obtain terephthalic acid DMF solution. Subsequently, mix the above two solutions and stir for 30min. Slowly add 10mL of acetic acid during stirring. After stirring, transfer the mixed solution to a stainless steel autoclave lined with polytetrafluoroethylene and hydroheat at 120℃ for 24h. After the reactor cools to room temperature, take out and collect the white precipitate by centrifugation. In a vacuum drying oven at 60℃ for 12h, UiO-66 white powder is obtained.
[0051] Step 2: 0.6 g of UiO-66 white powder and 0.2 g of PVP in step 1 were placed in a conical flask filled with deionized water and ultrasonicated for 15 minutes to obtain a uniform dispersion;
[0052] Step 3: Dissolve 42 mg of RuCl3·xH2O in the dispersion, stir magnetically for 30 min, and then add ammonia water dropwise during stirring until the pH is 10. After stirring, transfer the conical flask containing the mixed solution to a water bath and stir at 60°C for 3 h. After the water bath, cool to room temperature and centrifuge, and wash with deionized water 3 times. Finally, transfer the washed sample to an oven and dry at 80°C for 12 h to obtain the MOF precursor of Ru / UiO-66.
[0053] Step 4: Place the precursor in a covered quartz crucible in a muffle furnace, heat it to a target temperature of 500°C at a rate of 5°C / min and maintain the constant temperature for 2 hours. After cooling, grind to obtain a dark green catalyst, recorded as 7wt% Ru / ZrO2.
[0054] Example 5
[0055] A method for preparing a metal particle Ru-loaded ZrO2 catalyst for catalytic synthesis of methane by hydrogenation of carbon dioxide comprises the following steps:
[0056] Step 1: Dissolve 5mM ZrCl4 in 30mL DMF and stir to obtain ZrCl4 DMF solution. Then dissolve 5mM in 30mL DMF and stir to obtain terephthalic acid DMF solution. Subsequently, mix the above two solutions and stir for 30min. Slowly add 10mL of acetic acid during stirring. After stirring, transfer the mixed solution to a stainless steel autoclave lined with polytetrafluoroethylene and hydroheat at 120℃ for 24h. After the reactor cools to room temperature, take out and collect the white precipitate by centrifugation. In a vacuum drying oven at 60℃ for 12h, UiO-66 white powder is obtained.
[0057] Step 2: 0.6 g of UiO-66 white powder and 0.2 g of PVP in step 1 were placed in a conical flask filled with deionized water and ultrasonicated for 15 minutes to obtain a uniform dispersion;
[0058] Step 3: Dissolve 54 mg of RuCl3·xH2O in the dispersion, stir magnetically for 30 min, and then add ammonia water dropwise during stirring until the pH is 10. After stirring, transfer the conical flask containing the mixed solution to a water bath and stir at 60°C for 3 h. After the water bath, cool to room temperature and centrifuge, and wash with deionized water 3 times. Finally, transfer the washed sample to an oven and dry at 80°C for 12 h to obtain the MOF precursor of Ru / UiO-66.
[0059] Step 4: Place the precursor in a covered quartz crucible in a muffle furnace, heat it to a target temperature of 500°C at a rate of 5°C / min and maintain the constant temperature for 2 hours. After cooling, grind to obtain a dark green catalyst, recorded as 9wt% Ru / ZrO2.
[0060] The catalysts prepared in different embodiments of the present invention were tested, and the XRD test diagram is shown in Figure 2. The X-ray diffraction peaks of UiO-66 match the standard spectrum, indicating that the MOF precursor is successfully synthesized. The X-ray diffraction peaks of ZrO2 powder have diffraction peaks consistent with those of tetragonal zirconium oxide (t-ZrO2, PDF#88-1007) and monoclinic zirconium oxide (m-ZrO2, PDF#72-1669), of which t-ZrO2 occupies the main part. In addition, Figure 2It can be seen from the figure that the diffraction peaks of RuO2 in the samples with different parameters are at 2θ=28.100°, 35.168° and 54.341°, respectively. It also has the (101) peak of t-ZrO2, and no other impurity diffraction peaks appear, indicating that the Ru / ZrO2 catalytic material was successfully composited.
[0061] The activity test of the catalyst xRu / ZrO2 (x=0.01, 0.03, 0.05, 0.07, 0.09) of Examples 1-5 was carried out. The specific test method and results are as follows:
[0062] The activity test of the above catalyst was carried out on a fixed bed reactor (quartz reaction tube with an inner diameter of 5mm). The catalyst loading was 0.05g mixed with 1g of quartz sand. Before the catalyst reaction, it was activated in 20mL / min of H2 gas at normal pressure for 1h. The reduction temperature was 300°C. When cooled to the reaction temperature of 100°C, a mixed gas with a volume ratio of H2:CO2 = 4:1 was introduced. The reaction pressure was 1MPa, and GHSV = 36000mL / (g·h). The reaction products were analyzed by gas chromatography, CO and CO2 were detected by TCD detector, and methane and other hydrocarbon gases were detected by FID detector. The content of each component in the tail gas was quantitatively analyzed using the corrected area normalization method. The activity test results are as follows Figure 1 As shown, from Figure 1 It can be seen that the 7wt% Ru / ZrO2 prepared in Experimental Example 4 exhibits good catalytic activity.
[0063] Figure 3 These are SEM and TEM images of the corresponding products in the preparation process of Example 4 of the present invention, wherein (a) and (b) are the prepared Zr-MOF (UiO-66), (c) is the 7% Ru / ZrO2 prepared in Example 4, (d) is the EDS element distribution diagram of Example 4, (e) is the element distribution diagram of Ru, (f) is the element distribution diagram of O, (g) is the element distribution diagram of Zr, and it can be seen from (dg) that the three elements Ru, O and Zr are evenly distributed on the catalyst and the Ru / ZrO2 catalyst is formed.
[0064] Finally, it should be noted that the above-mentioned embodiments only express several implementation methods of the present invention and are not intended to limit the invention. For those skilled in the art, any modification, equivalent replacement, improvement, etc. made without departing from the concept of the present invention should be included in the protection scope of the invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A UiO-66 derived Ru / ZrO2 catalyst, characterized in that: The Ru / ZrO2 catalyst is obtained by in-situ growth of metal particles of Ru on the surface of octahedral ZrO2 derived from UiO-66 and calcination.
2. The Ru / ZrO2 catalyst derived from UiO-66 according to claim 1, characterized in that The preparation method of Ru / ZrO2 catalyst comprises the following steps: Step 1: dissolving ZrCl4 in DMF and stirring evenly to obtain a ZrCl4DMF solution; dissolving terephthalic acid in the DMF solution at room temperature, and then mixing it with the ZrCl4DMF solution, and continuing to stir. During the stirring process, slowly dropwise adding acetic acid, after the stirring is completed, transferring the mixed solution to a stainless steel autoclave lined with polytetrafluoroethylene for hydrothermal reaction, after the reaction is completed, the autoclave is cooled to room temperature, taken out and centrifuged to collect the white precipitate, washed, dried, and ground to obtain white UiO-66 powder; Step 2: Place the white UiO-66 powder and PVP in a conical flask filled with deionized water and sonicate to obtain a uniform dispersion; Step 3: Dissolve RuCl3·xH2O in the dispersion, stir magnetically, add ammonia water dropwise during stirring until the pH is 10, continue heating and stirring in a water bath after stirring, wait until it cools to room temperature, centrifuge, wash, and dry to obtain a MOF precursor of Ru / UiO-66; Step 4: Place the MOF precursor of Ru / UiO-66 in a covered quartz crucible in a muffle furnace, calcine, and grind after cooling to obtain a dark green Ru / ZrO2 catalyst.
3. The Ru / ZrO2 catalyst derived from UiO-66 according to claim 2, characterized in that In step 1, the molar ratio of ZrCl4 to terephthalic acid is 1:1; the volume ratio of DMF to acetic acid is 6:
1.
4. The Ru / ZrO2 catalyst derived from UiO-66 according to claim 2, characterized in that In step 1, the hydrothermal reaction temperature is 120° C. and the reaction time is 24 h.
5. The Ru / ZrO2 catalyst derived from UiO-66 according to claim 2, characterized in that The mass ratio of UiO-66 powder to PVP in step 2 is 3:
1.
6. The Ru / ZrO2 catalyst derived from UiO-66 according to claim 2, characterized in that In step 3, the mass ratio of RuCl3·xH2O and UiO-66 powder is 0.01-0.09:
1.
7. The Ru / ZrO2 catalyst derived from UiO-66 according to claim 2, characterized in that In step 3, the water bath heating stirring temperature is 60° C. and the stirring time is 3 h.
8. The Ru / ZrO2 catalyst derived from UiO-66 according to claim 2, characterized in that In step 4, the calcination temperature is 500° C., and a temperature program is set at a rate of 5° C. / min. After the temperature reaches 500° C., the temperature is kept constant for 2 hours.
9. Use of the Ru / ZrO2 catalyst derived from UiO-66 as claimed in any one of claims 1 to 8 in the hydrogenation of carbon dioxide to produce methane, characterized in that: The reaction raw gas used is composed of CO2 and H2.
10. The use according to claim 9, characterized in that: The flow rate ratio of CO2 and H2 is 1:3-4, the reaction temperature is 170-250°C, and the reaction pressure is 0.5-1.5MPa.
Citation Information
Patent Citations
Preparation method of CO selective methanation catalyst
CN101607200A
Preparation method of composite metal material catalyst and application of composite metal material catalyst in preparation of 5-HMF
CN111617771A