Method for preparing copper-zinc-aluminum catalyst with assistance of Joule thermal pulse and copper-zinc-aluminum catalyst
Through the Joule thermal pulse assisted preparation method, the problems of particle size adjustment and sintering inactivation of copper-zinc-aluminum catalysts were solved, and a catalyst with small particle size and high activity was prepared, which significantly improved its catalytic performance in methanol synthesis.
Patent Information
- Application Number
- CN202411070266.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
AI Technical Summary
The particle size of copper-zinc-aluminum catalysts is not easy to adjust and sintering inactivation is still a practical problem that needs to be solved urgently. Traditional roasting and heating methods often cannot effectively regulate the grains of the active components of the catalyst.
The Joule thermal pulse assisted preparation method is adopted to control multi-period instantaneous cooling through pulse power supply, promote structural changes of the catalyst precursor, and quickly cool down to inhibit grain growth, obtain anti-sintered copper-zinc-aluminum with small particle size and high specific surface area. catalyst.
The prepared catalyst has a smaller Cu-Zn particle size, higher Cu-Zn interface activity, good anti-sintering performance, and excellent catalytic performance in the hydrogenation of CO or CO2 to methanol.
Smart Images

Figure CN118988329A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of methanol synthesis, and in particular to a method for preparing a copper-zinc-aluminum catalyst assisted by Joule heat pulse and the copper-zinc-aluminum catalyst. Background Art
[0002] Copper-zinc-aluminum catalysts are currently important hydrogenation and dehydrogenation catalysts in industry and can be used to catalyze CO x Reactions such as hydrogenation to methanol, CO and steam shift to hydrogen, methanol cracking, etc. In recent years, the energy conversion problem under the dual-carbon background has prompted copper-zinc-aluminum catalysts to become a research hotspot again. Among them, the combination of new catalyst preparation methods and traditional catalyst preparation methods is an important idea for developing low-cost and more efficient copper-zinc-aluminum catalysts.
[0003] The catalyst is generally prepared by coprecipitation, through the precipitation reaction of salt solution of copper nitrate, zinc nitrate, aluminum nitrate and other additives with the precipitant, a uniform precipitate is obtained, i.e., the precursor of the catalyst. In the coprecipitation method, the preparation conditions such as precipitation method, precipitation order, precipitation temperature, and roasting conditions are important factors affecting the structure of the catalyst. Researchers often improve the dispersion of copper, the specific surface area of the catalyst, the grain size and the sintering resistance by adjusting the preparation conditions. Patent CN106179360B adds an organic solvent to the solution of the precipitant, and first precipitates the copper-zinc precipitate and then precipitates the aluminum precipitate. The pore size of the copper-zinc-aluminum catalyst prepared by the patent CN106179360B is 9 to 15 nm, and it has higher activity and better heat resistance in the application of CO low-temperature shift hydrogen production process. CN115228477B embeds active components into a carbon coating layer to form a carbon-coated nanoflower-like structure catalyst, which can improve the activity and hydrothermal stability of the catalyst and reduce the metal particle size. However, the particle size of the copper-zinc-aluminum catalyst is difficult to adjust, and sintering deactivation is still a practical problem that needs to be solved urgently. Traditional roasting and heating methods often cannot effectively regulate the grain size of the active components of the catalyst.
[0004] The preparation of catalysts assisted by Joule heat pulses is a promising method for preparing catalysts. Based on the principle of Joule heating effect, the pulse power source controls the instantaneous temperature rise and fall of multiple cycles. When the current passes through the conductive carbon felt, it generates instantaneous high temperature to promote the structural change of the catalyst precursor. In addition, rapid cooling inhibits the growth of grains, thereby preparing a sintering-resistant copper-zinc-aluminum catalyst with small particle size and high specific surface area. This method can also shorten the catalyst roasting time, which is conducive to energy saving.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a method for preparing a copper-zinc-aluminum catalyst assisted by Joule heat pulse, which overcomes the defects of poor dispersibility and easy sintering of active components in existing copper-zinc-aluminum catalysts.
[0007] The main ideas of the technical solution of the present invention are as follows: A method for preparing a copper-zinc-aluminum catalyst assisted by Joule heat pulse comprises the following steps: (1) preheating a copper salt solution, a zinc salt solution and a precipitant solution to a precipitation temperature, and then adding them dropwise into a precipitation container, and performing precipitation and aging to obtain a mixed slurry I; (2) adding the aluminum salt solution, the modification aid and the precipitant to the mixed slurry I, stirring and mixing, to obtain a mixed slurry II; (3) After aging the mixed slurry II, filtering, washing, and then drying to obtain a dry material; (4) Taking an appropriate amount of dry material and placing it in a Joule heat pulse reactor, and subjecting it to pulse treatment under an inert gas atmosphere, the copper-zinc-aluminum catalyst is obtained.
[0008] As a method, the concentrations of the copper salt solution, zinc salt solution and precipitant solution are 0.5-1.5 mol L -1 .
[0009] As one embodiment, the precipitating agent is an inorganic base, preferably sodium carbonate.
[0010] As a method, in step (1), the precipitation temperature is 35-85°C; preferably, the dripping rate is 5-25 mL min -1 .
[0011] As one method, in step (2), the aluminum salt solution is an aluminum nitrate solution with a concentration of 0.5-1.5 mol L -1 .
[0012] Preferably, the modification aid is a magnesium salt or a silicon salt solution.
[0013] Preferably, the rate of adding the mixed slurry I is 5-25 mL min -1 .
[0014] As a method, in step (4), the inert gas is Ar, N2 or He, the heating form is pulse, and the pulse conditions are: the Joule heat high temperature is 400-1000°C, more preferably 800-1000°C; the number of pulse discharges is 3-15 times.
[0015] As a method, the heating rate is 2000-4000℃ / s, the cooling time is ≤1.5s, and it drops to 400℃±10℃ before the next pulse process.
[0016] The present invention also provides a copper-zinc-aluminum catalyst, which is prepared by any of the methods described above.
[0017] The present invention further provides a method for synthesizing methanol, which adopts the copper-zinc-aluminum catalyst described in the present invention.
[0018] The present invention has the following advantages: 1. The Joule heat pulse assisted preparation method of copper-zinc-aluminum catalyst of the present invention controls the instantaneous temperature rise and fall of multiple cycles by pulse power supply. When the current passes through the conductive carbon felt, the instantaneous high temperature is generated to promote the structural change of the catalyst precursor, and the rapid cooling inhibits the growth of grains. The obtained catalyst has a smaller Cu-Zn particle size, higher Cu-Zn interface activity, and good anti-sintering performance. The particle size of the active component is 3-6nm, the specific surface area of the copper-zinc-aluminum catalyst is ≥160m2 / g, and the pore size is 8-15nm.
[0019] 2. The copper-zinc-aluminum catalyst prepared by the present invention has demonstrated excellent catalytic performance in the actual evaluation of CO or CO2 hydrogenation to methanol, and at the same time provides ideas for the preparation of nano metal oxide catalysts. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The accompanying drawings are used to provide a further understanding of the technical solution of the present invention and constitute a part of the specification. Together with the embodiments of the present application, they are used to explain the technical solution of the present invention and do not constitute a limitation on the technical solution of the present invention.
[0021] Figure 1 It is the XRD diagram of the catalysts prepared in Examples 1-5 of the present invention and Comparative Examples 1-2.
[0022] Figure 2 This is a TEM image of the catalyst of Example 5 of the present invention.
[0023] Figure 3 This is the EDX elemental analysis diagram of the catalyst of Example 5 of the present invention. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The concentrations of the zinc salt solution, copper salt solution, and aluminum salt solution used in Examples 1-5 below were 1.25 mol L -1The concentration of the precipitant Na2CO3 solution is 1.25 mol L -1 ; The concentration of Mg(NO3)2 solution is 1.25 mol L -1 ; The Na2SiO3 solution is a self-purchased Na2SiO3 solution with a silicon content of 12%-13% (mass percentage).
[0026] Example 1 (1) 50 mL Zn(NO3)2 solution, 100 mL Cu(NO3)2 solution, and 190 mL Na2CO3 solution were pumped at 80 °C at a rate of 18 mL min -1 The mixture was added into the precipitation container at a dropping rate of , and aged at 80°C for 30min to obtain a mixed slurry I; (2) Then, 17 mL of Al(NO3)3 solution, 4 mL of Mg(NO3)2 solution, 0.85 mL of Na2SiO3 solution, and 25 mL of Na2CO3 solution were pumped at 18 mL min-1. -1 The Cu-Zn-Al slurry is simultaneously pumped into the mixed slurry I at a dropping rate to obtain a mixed slurry II (Cu-Zn-Al slurry); (3) The mixed slurry II was aged at 80° C. for 50 min, then washed and filtered to obtain a wet material, and the wet material was dried at 110° C. for 12 h to obtain a dry material; (4) Take 2g of the dry material obtained in step (3) and place it in a carbon cloth, clamp the two ends with copper sheets, and use a multimeter to measure the resistance of the two ends of the carbon cloth. Replace the air in the sintering box with monatomic gas Ar, set the pulse conditions: the heating rate is 3000℃ / s, the number of pulses is 5 times, the upper limit temperature is 800℃, the cooling time is 1.5s, and it drops to 400℃±10℃; after the pulse ends, the catalyst powder is obtained, and then the catalyst is pressed into tablets; when pressing, weigh 4g of catalyst powder into the mold each time, the pressure is 20MPa, the time is 5min, and the catalyst particles are retained at 20-40 mesh for standby use.
[0027] Example 2 (1) 50 mL Zn(NO3)2 solution, 100 mL Cu(NO3)2 solution, and 190 mL Na2CO3 solution were pumped at 80 °C at a rate of 18 mL min -1 The mixture was added into the precipitation container at a dropping rate of , and aged at 80°C for 30min to obtain a mixed slurry I; (2) Then, 17 mL of Al(NO3)3 solution, 4 mL of Mg(NO3)2 solution, 0.85 mL of Na2SiO3 solution, and 25 mL of Na2CO3 solution were pumped at 18 mL min-1. -1The Cu-Zn-Al slurry is simultaneously pumped into the mixed slurry I at a dropping rate to obtain a mixed slurry II (Cu-Zn-Al slurry); (3) The mixed slurry II was aged at 80° C. for 50 min, then washed and filtered to obtain a wet material, and the wet material was dried at 110° C. for 12 h to obtain a dry material; (4) Take 2g of the dry material obtained in step (3) and place it in a carbon cloth, clamp the two ends with copper sheets, and use a multimeter to measure the resistance of the two ends of the carbon cloth. Replace the air in the sintering box with monatomic gas Ar, set the pulse conditions: the heating rate is 2000℃ / s, the number of pulses is 15 times, the upper limit temperature is 800℃, the cooling time is 1.5s, and it drops to 400℃±10℃; after the pulse ends, the catalyst powder is obtained, and then the catalyst is pressed into tablets; when pressing, weigh 4g of catalyst powder into the mold each time, the pressure is 20MPa, the time is 5min, and the catalyst particles are retained at 20-40 mesh for standby use.
[0028] Example 3 (1) Prepare 50 mL Zn(NO3)2 solution, 100 mL Cu(NO3)2 solution, and 190 mL Na2CO3 solution at 80 °C using a peristaltic pump at a rate of 18 mL min -1 The mixture was added into the precipitation container at a dropping rate of , and aged at 80°C for 30min to obtain a mixed slurry I; (2) Then, 17 mL of Al(NO3)3 solution, 4 mL of Mg(NO3)2 solution, 0.85 mL of Na2SiO3 solution, and 25 mL of Na2CO3 solution were pumped at 18 mL min-1. -1 The Cu-Zn-Al slurry is simultaneously pumped into the mixed slurry I at a dropping rate to obtain a mixed slurry II (Cu-Zn-Al slurry); (3) The mixed slurry II was aged at 80° C. for 50 min, then washed and filtered to obtain a wet material, and the wet material was dried at 110° C. for 12 h to obtain a dry material; (4) Take 2g of the dry material obtained in step (3) and place it in a carbon cloth, clamp the two ends with copper sheets, and use a multimeter to measure the resistance of the two ends of the carbon cloth. Replace the air in the sintering box with monatomic gas Ar, set the pulse conditions: the heating rate is 3000℃ / s, the number of pulses is 15 times, the upper limit temperature is 800℃, the cooling time is 1.5s, and it drops to 400℃±10℃; after the pulse ends, the catalyst powder is obtained, and then the catalyst is pressed into tablets; when pressing, weigh 4g of catalyst powder into the mold each time, the pressure is 20MPa, the time is 5min, and the catalyst particles are retained at 20-40 mesh for standby use.
[0029] Example 4 (1) Prepare 50 mL Zn(NO3)2 solution, 100 mL Cu(NO3)2 solution, and 190 mL Na2CO3 solution at 80 °C using a peristaltic pump at a rate of 18 mL min -1 The mixture was added into the precipitation container at a dropping rate of , and aged at 80°C for 30min to obtain a mixed slurry I; (2) Then, 17 mL of Al(NO3)3 solution, 4 mL of Mg(NO3)2 solution, 0.85 mL of Na2SiO3 solution, and 1.25 M 25 mL of Na2CO3 solution were pumped at 18 mL min -1 The Cu-Zn-Al slurry is simultaneously pumped into the mixed slurry I at a dropping rate to obtain a mixed slurry II (Cu-Zn-Al slurry); (3) The mixed slurry II was aged at 80° C. for 50 min, then washed and filtered to obtain a wet material, and the wet material was dried at 110° C. for 12 h to obtain a dry material; (4) Take 2g of the dry material obtained in step (3) and place it in a carbon cloth, clamp the two ends with copper sheets, and use a multimeter to measure the resistance of the two ends of the carbon cloth. Replace the air in the sintering box with monatomic gas Ar, set the pulse conditions: the heating rate is 2000℃ / s, the number of pulses is 15 times, the upper limit temperature is 1000℃, the cooling time is 1.5s, and it drops to 400℃±10℃; after the pulse ends, the catalyst powder is obtained, and then the catalyst is pressed into tablets; when pressing, weigh 4g of catalyst powder into the mold each time, the pressure is 20MPa, the time is 5min, and the catalyst particles are retained at 20-40 mesh for standby use.
[0030] Example 5 (1) Prepare 50 mL Zn(NO3)2 solution, 100 mL Cu(NO3)2 solution, and 190 mL Na2CO3 solution at 80 °C using a peristaltic pump at a rate of 18 mL min -1 The mixture was added into the precipitation container at a dropping rate of , and aged at 80°C for 30min to obtain a mixed slurry I; (2) Then, 17 mL of Al(NO3)3 solution, 4 mL of Mg(NO3)2 solution, 0.85 mL of Na2SiO3 solution, and 25 mL of Na2CO3 solution were pumped at 18 mL min-1. -1 The Cu-Zn-Al slurry is simultaneously pumped into the mixed slurry I at a dropping rate to obtain a mixed slurry II (Cu-Zn-Al slurry); (3) The mixed slurry II was aged at 80° C. for 50 min, then washed and filtered to obtain a wet material, and the wet material was dried at 110° C. for 12 h to obtain a dry material; (4) Take 2g of the dry material obtained in step (3) and place it in a carbon cloth, clamp the two ends with copper sheets, and use a multimeter to measure the resistance of the two ends of the carbon cloth. Replace the air in the sintering box with monatomic gas Ar, set the pulse conditions: the heating rate is 3000℃ / s, the number of pulses is 15 times, the upper limit temperature is 1000℃, the cooling time is 1.5s, and it drops to 400℃±10℃; after the pulse ends, the catalyst powder is obtained, and then the catalyst is pressed into tablets; when pressing, weigh 4g of catalyst powder into the mold each time, the pressure is 20MPa, the time is 5min, and the catalyst particles are retained at 20-40 mesh for standby use.
[0031] Comparative Example 1 Comparative Example 1 is a catalyst prepared without the assistance of Joule heat pulse, which is a catalyst prepared by a conventional method. The specific steps are as follows: (1) 50 mL Zn(NO3)2 solution, 100 mL Cu(NO3)2 solution, and 190 mL Na2CO3 solution were prepared at 80°C by a peristaltic pump at a rate of 18 mL min -1 The mixture was added into the precipitation container at a dropping rate of , and aged at 80°C for 30min to obtain a mixed slurry I; (2) Then, 17 mL of Al(NO3)3 solution, 4 mL of Mg(NO3)2 solution, 0.85 mL of Na2SiO3 solution, and 25 mL of Na2CO3 solution were pumped at 18 mL min-1. -1 The Cu-Zn-Al slurry is simultaneously pumped into the mixed slurry I at a dropping rate to obtain a mixed slurry II (Cu-Zn-Al slurry); (3) The mixed slurry II is aged at 80°C for 50 min. The wet material is then washed and filtered to obtain a dry material, which is then dried at 110°C for 12 h to obtain a dry material; (4) Take 2 g of the dry material from step (3) and place it in a crucible at 5 °C min -1 The catalyst was calcined at 350°C for 3 h at a heating rate of 1.5 °C and then pressed into tablets. When pressing, 2 g of catalyst powder was weighed into a mold each time. The pressure was 20 MPa and the time was 5 min. The catalyst particles were retained at 20-40 mesh for later use.
[0032] Comparative Example 2 A domestic commercial catalyst. In order to avoid adversely affecting the sales of other people's products, the product information is hidden. The component comparison between the commercial catalyst and the catalyst of Example 5 of the present invention is shown in Table 1 (XRF element composition table).
[0033] Table 1 The XRD patterns of the catalysts prepared in Examples 1-5 and Comparative Examples 1-2 are as follows: Figure 1As shown. The particle size of the catalyst components was characterized by XRD. The particle size of the catalyst prepared by Joule heat pulse in Examples 1-5 was significantly smaller than that of the commercial catalyst and the catalyst prepared by conventional precipitation method. By changing the Joule heating conditions, the catalyst prepared by faster heating and cooling rate and appropriate pulse number can form a catalyst with smaller particle size.
[0034] Figure 2 This is a TEM image of the catalyst of Example 5. Analysis of this image shows that the grain size of the catalyst prepared by Joule heat pulse meets the expected target and is generally distributed around 5 nm.
[0035] Figure 3 This is the EDX elemental analysis diagram of the catalyst of Example 5 of the present invention. From the EDX elemental analysis diagram, it can be found that each element is evenly distributed on the catalyst, indicating that the dispersion of each component is good.
[0036] Effect Example 1 Catalyst reduction conditions: Reduction gas composition: 5% H2 + 95% N2, reduction space velocity 5000h -1 , pressure 0.8MPa.
[0037] Catalyst reaction conditions: reaction mixture composition is 8.00% Ar + 89.24% CO + 2.26% CO2, catalyst particle size is 20-40 mesh, volume is 1 mL, pressure is 5 MPa, temperature is 250 ° C, space velocity is 10000 h -1 The flow rate during the reaction was 116.67 mL min-1 for H2. -1 The reaction mixture flow rate is 50 mL min -1 .
[0038] The liquid product was sampled once every 3 hours, weighed and the yield was calculated. After three samplings, the heat resistance procedure was started, the temperature was raised to 380°C and maintained for 5 hours. After the heat resistance was completed, the temperature was lowered to 250°C and the evaluation was continued for 6 hours. The heat resistance retention rate was the ratio of the liquid phase yield of the catalyst before and after heat resistance.
[0039] Analysis method: Quantitative detection by gas chromatography, automatic injection, carrier gas is H2, pneumatic valve drive gas is N2, chromatographic column is TDX-01, chromatographic column for liquid product analysis is Porapak Q, TCD detector, injection port temperature is 120℃, column temperature is 90℃, detector temperature is 150℃, bridge current is 100mA, carrier gas flow rate is 60mL min -1 .
[0040] The CO conversion rate was detected by the internal standard method, and the selectivity of products such as methanol in the product was determined by the area normalization method. The carbon balance was used to analyze and quantitatively calculate the C of the reaction process, and the external standard method was used to assist the calculation.
[0041] The catalytic performance of the catalyst in the synthesis gas to methanol process is shown in Table 2. CO , % represents the conversion rate of CO.
[0042] The results in Table 2 show that the catalyst prepared with the assistance of Joule heat pulse has excellent catalytic performance in the methanol synthesis process, such as high CO conversion rate, methanol space-time yield and heat resistance retention rate. This is mainly due to the fact that the catalyst prepared with the assistance of Joule heat pulse has a smaller particle size and better dispersion of active components than commercial catalysts and catalysts prepared by conventional precipitation methods.
[0043] Table 2
[0044] Although the embodiments disclosed in the present invention are as above, the contents described are only embodiments adopted to facilitate understanding of the present invention and are not intended to limit the present invention. Any technician in the field to which the present invention belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in the present invention, but the patent protection scope of the present invention shall still be subject to the scope defined in the attached claims.
Claims
1. A method for preparing a copper-zinc-aluminum catalyst assisted by Joule heat pulse, comprising the following steps: (1) Preheat the copper salt solution, zinc salt solution and precipitant solution to the precipitation temperature, then add them dropwise into the precipitation container, and after precipitation and aging, obtain a mixed slurry. ; (2) Add aluminum salt solution, modification aid and precipitant to the mixed slurry Mix by stirring to obtain a mixed slurry ; (3) Mix the slurry After aging, the product is filtered, washed, and then dried to obtain a dry material; (4) Taking an appropriate amount of dry material and placing it in a Joule heat pulse reactor, and subjecting it to pulse treatment under an inert gas atmosphere, the copper-zinc-aluminum catalyst is obtained.
2. The method for preparing copper-zinc-aluminum catalyst assisted by Joule heat pulse according to claim 1, characterized in that: The concentrations of the copper salt solution, zinc salt solution and precipitant solution are 0.5-1.5 mol L -1 .
3. The method for preparing copper-zinc-aluminum catalyst assisted by Joule heat pulse according to claim 1, characterized in that: The precipitating agent is an inorganic base, preferably sodium carbonate.
4. The method for preparing copper-zinc-aluminum catalyst assisted by Joule heat pulse according to claim 1, characterized in that: In step (1), the precipitation temperature is 35-85°C; preferably, the dropwise addition rate is 5-25 mL min -1 .
5. The method for preparing copper-zinc-aluminum catalyst assisted by Joule heat pulse according to claim 1, characterized in that: In step (2), the aluminum salt solution is aluminum nitrate solution with a concentration of 0.5-1.5 mol L -1 ; Preferably, the modification aid is a magnesium salt or a silicon salt solution; Preferably, the mixed slurry is added The rate is 5-25 mL min -1 .
6. The method for preparing copper-zinc-aluminum catalyst assisted by Joule heat pulse according to claim 1, characterized in that: In step (4), the inert gas is Ar, N2 or He, and the heating form is pulsed; Preferably, the pulse conditions are: the Joule heat high temperature is 400-1000° C., more preferably 800-1000° C.; and the number of pulse discharges is 3-15 times.
7. The method for preparing copper-zinc-aluminum catalyst assisted by Joule heat pulse according to claim 6, characterized in that: The heating rate is 2000-4000℃ / s, the cooling time is ≤1.5s, and it drops to 400℃±10℃ before the next pulse process.
8. A copper-zinc-aluminum catalyst, characterized in that The method is prepared by any one of claims 1 to 7.
9. A method for synthesizing methanol, characterized in that: The copper-zinc-aluminum catalyst as claimed in claim 8 is used.
Citation Information
Patent Citations
Copper-zinc-aluminum catalyst and preparation method thereof
CN106179360A
Ni-based high-entropy compound catalyst for methane reforming process as well as preparation method and application of Ni-based high-entropy compound catalyst
CN118059882A
Copper-based catalyst as well as preparation method and application thereof
CN118079932A