Bismuth vanadate / iron vanadate composite acoustic catalyst as well as preparation method and application thereof

Through the heterojunction structure of bismuth vanadate/ferrous vanadate composite acoustic catalyst, the acoustic catalytic activity of BiVO4 is improved, the problem of low acoustic catalytic efficiency of BiVO4 is solved, and the efficient removal of tetracycline pollutants in the water environment is achieved. Stable and environmentally friendly characteristics.

CN118988337AActive Publication Date: 2024-11-22LIAONING UNIVERSITY

Patent Information

Application Number
CN202411082418.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The acoustic catalytic activity of BiVO4 is limited by its high-light induced recombination degree and insufficient surface adsorption characteristics, resulting in low acoustic catalytic efficiency and it is difficult to effectively remove tetracycline pollutants in the water environment.

Method used

BiVO4/FeVO4 composite material is prepared by hydrothermal synthesis method using bismuth vanadate/ferrous vanadate composite acoustic catalyst to form a heterojunction structure to improve the separation efficiency of electron hole pairs, thereby improving the efficiency of acoustic catalytic removal of tetracycline.

Benefits of technology

Through the use of bismuth vanadate/ferrous vanadate composite acoustic catalyst, the acoustic catalytic activity is significantly improved, and a more efficient tetracycline removal effect is achieved, with a removal rate of up to 94.80±1.09%, and it is chemically and thermally stable and non-toxic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988337A_ABST
    Figure CN118988337A_ABST
Patent Text Reader

Abstract

The invention discloses a bismuth vanadate / iron vanadate composite acoustic catalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: dissolving Bi (NO3) 3.5 H2O and Fe (NO3) 3.9 H2O in a nitric acid solution, uniformly mixing, slowly dropwise adding a NaOH solution of NH4VO3, adjusting the pH value of the solution, uniformly stirring, transferring the mixed solution into a reaction kettle, carrying out a hydrothermal synthesis reaction, cooling to room temperature, carrying out suction filtration, washing, drying, and carrying out high-temperature calcination in a tubular furnace to obtain the bismuth vanadate / iron vanadate composite acoustic catalyst BiVO4 / FeVO4. The composite material provided by the invention has a synergistic effect with potassium persulfate to remove tetracycline through ultrasonic catalysis, the removal efficiency is high, and the reaction time is short. By using the method, the removal rate of tetracycline can reach 94.80% under the ultrasonic condition for 120 minutes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of acoustic catalytic composite materials, and in particular relates to a bismuth vanadate / iron vanadate composite acoustic catalyst and a preparation method and application thereof. Background Art

[0002] Tetracyclines are widely used in human and animal therapeutic applications due to their broad spectrum, high efficacy, and reasonable cost. However, the high stability of tetracyclines leads to the release of tetracycline residues into aquatic environments. The presence of tetracyclines in the environment can hinder soil microbial functions and can also cause toxic or teratogenic effects on plants and animals. In addition, it also contributes to the emergence and spread of resistance genes (ARGs) and drug-resistant bacteria (ARBs). Considering the difficulty of tetracycline removal in aquatic environments, it is necessary to develop effective methods to remove tetracycline.

[0003] There are many processes for removing tetracycline from wastewater, such as adsorption, electrolysis, photocatalysis, and chemical oxidation. As an advanced chemical oxidation method, acoustic catalysis has a good wastewater treatment effect. In the ultrasonic process, bubbles are formed by cavitation, and the bubble rupture produces sonoluminescence (SL) and high temperature and high pressure, thereby generating a lot of active oxygen to mineralize organic matter. In addition, the addition of acoustic catalysts can further improve the efficiency of acoustic catalytic removal by generating electron-hole pairs.

[0004] BiVO4 is a semiconductor material with a small band gap, which enables it to effectively absorb visible light and generate electron-hole pairs required for photocatalysis. Among them, monoclinic scheelite BiVO4 has been proven to be an efficient photocatalyst, which not only has the characteristics of low manufacturing cost, low hazard, and good photostability, but also is a very promising material. However, although the photocatalytic and sonocatalytic mechanisms are similar, the sonocatalytic activity of BiVO4 is limited by its high light-induced recombination degree and insufficient surface adsorption characteristics, resulting in low sonocatalytic efficiency. Summary of the invention

[0005] The present invention aims to provide a bismuth vanadate / iron vanadate composite acoustic catalyst, which utilizes bismuth vanadate and iron vanadate to form a heterojunction to improve the separation efficiency of electron-hole pairs, thereby improving the acoustic catalytic removal of tetracycline pollutants.

[0006] The technical scheme adopted by the present invention is: a bismuth vanadate / iron vanadate composite acoustic catalyst, and the preparation method comprises the following steps: taking Bi(NO3)3·5H2O and Fe(NO3)3·9H2O, adding nitric acid solution to dissolve, mixing evenly, slowly dropping NH4VO3 NaOH solution, adjusting the solution pH, stirring evenly, transferring the mixed solution to a reactor for hydrothermal synthesis reaction, cooling to room temperature, filtering, washing, drying, and calcining at high temperature in a tubular furnace to obtain a bismuth vanadate / iron vanadate composite acoustic catalyst (BiVO4 / FeVO4).

[0007] Furthermore, in molar ratio, Bi(NO3)3·5H2O:Fe(NO3)3·9H2O=10:(2~7).

[0008] Furthermore, in molar ratio, Bi(NO3)3·5H2O:NH4VO3=10:(12~17).

[0009] Furthermore, the pH of the solution is adjusted to 1.5-2.5.

[0010] Furthermore, the hydrothermal synthesis reaction is carried out at 175-185° C. for 22-26 hours.

[0011] Furthermore, the high temperature calcination is performed at a calcination temperature of 450 to 550° C., a calcination holding time of 4 to 5 hours, and a heating rate of 5° C. / min.

[0012] The invention provides an application of a bismuth vanadate / iron vanadate composite sonic catalyst in catalytic removal of organic pollutants.

[0013] Furthermore, the organic pollutant is tetracycline.

[0014] Furthermore, the method is as follows: adding bismuth vanadate / iron vanadate composite acoustic catalyst into wastewater containing tetracycline and ultrasonicating.

[0015] Furthermore, the addition amount of the bismuth vanadate / iron vanadate composite sonic catalyst is 1.0-1.5 mg / mL, the concentration of tetracycline is 40-60 mg / L, the ultrasonic power is 500 W, and the ultrasonic time is 100-150 min.

[0016] Furthermore, potassium persulfate is added simultaneously.

[0017] Furthermore, the amount of potassium persulfate added is 0.25 to 3.0 mg / mL.

[0018] The beneficial effects of the present invention are:

[0019] The present invention combines FeVO4 and BiVO4 to form a heterojunction structure. As a semiconductor photocatalyst, FeVO4 has the advantages of ultraviolet visible light drive, small band gap, chemical and thermal stability, and non-toxicity, and can effectively promote the separation and migration of electron-hole pairs, generating a strong hole oxidation ability. The present invention greatly improves the sonocatalytic activity by combining FeVO4 and BiVO4 to form a heterojunction structure, thereby achieving a more efficient sonocatalytic process.

[0020] The iron vanadate / bismuth vanadate composite sonic catalytic material of the present invention utilizes the good catalytic performance of bismuth vanadate and iron vanadate, and their composite produces a synergistic effect, thereby improving the catalytic efficiency and reaction rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the XPS spectrum of the prepared BiVO4 / FeVO4 composite material.

[0022] Figure 2 This is a diagram showing the effect of BiVO4 / FeVO4 composite materials prepared with different composite ratios on the removal effect of tetracycline solution.

[0023] Figure 3 This is a diagram showing the effect of ultrasonic catalysis in removing tetracycline using a BiVO4 / FeVO4 composite material with a composite ratio of 60% and different amounts of potassium persulfate added. DETAILED DESCRIPTION

[0024] Example 1 Bismuth vanadate / iron vanadate composite acoustic catalyst (BiVO4 / FeVO4)

[0025] (I) BiVO4 / FeVO4 with a composite ratio of 20%

[0026] The preparation method is as follows:

[0027] Weigh Fe(NO3)3·9H2O (808 mg, 2 mmol) and Bi(NO3)3·5H2O (4850.7 mg, 10 mmol), dissolve in 2 mL of concentrated nitric acid, then add deionized water to dilute to 20 mL, and after magnetic stirring for a period of time, obtain a clear solution A. Weigh NH4VO3 (1404 mg, 12 mmol) and dissolve in 20 mL of 2 mol / L NaOH solution to obtain solution B. Under stirring, add solution B dropwise to solution A to form a yellow solution, then adjust the pH value of the mixed solution to 2 with 2 mol / L NaOH solution and continue magnetic stirring for 30 min after stabilization. Transfer the resulting mixture to a polytetrafluoroethylene reactor, place it in a forced air drying oven, and react at 180 ° C for 24 h; cool to room temperature and filter, rinse the filter residue three times with deionized water, and then wash it three times with anhydrous ethanol. Finally, the product was placed in a vacuum drying oven to dry, dried at 60°C for 6 hours, then ground and calcined at 500°C in a tubular furnace for 4 hours (heating rate of 5°C / min) to obtain a BiVO4 / FeVO4 composite material with a molar ratio of Bi(NO3)3·5H2O:Fe(NO3)3·9H2O=10:2 and a Fe(NO3)3·9H2O composite ratio of 20%.

[0028] (ii) BiVO4 / FeVO4 with a composite ratio of 30%

[0029] The preparation method is as follows:

[0030] Fe(NO3)3·9H2O (1212 mg, 3 mmol) and Bi(NO3)3·5H2O (4850.7 mg, 10 mmol) were weighed and dissolved in 2 mL of concentrated nitric acid, then deionized water was added to dilute to 20 mL, and after magnetic stirring for a period of time, a clear solution A was obtained. NH4VO3 (1521 mg, 13 mmol) was weighed and dissolved in 20 mL of 2 mol / L NaOH solution to obtain solution B. Under stirring, solution B was added dropwise to solution A to form a yellow solution, and then the pH value of the mixed solution was adjusted to 2 with 2 mol / L NaOH solution and stabilized, and then magnetic stirring was continued for 30 min. The obtained mixture was transferred to a polytetrafluoroethylene reactor, placed in a forced air drying oven, and reacted at 180 ° C for 24 h; after cooling to room temperature, it was filtered, and the filter residue was rinsed three times with deionized water, and then washed three times with anhydrous ethanol. Finally, the product was placed in a vacuum drying oven to dry, dried at 60°C for 6 hours, then ground and calcined at 500°C in a tubular furnace for 4 hours (heating rate of 5°C / min) to obtain a BiVO4 / FeVO4 composite material with a molar ratio of Bi(NO3)3·5H2O:Fe(NO3)3·9H2O=10:3 and a Fe(NO3)3·9H2O composite ratio of 30%.

[0031] (III) BiVO4 / FeVO4 with a composite ratio of 40%

[0032] The preparation method is as follows:

[0033] Weigh Fe(NO3)3·9H2O (1616 mg, 4 mmol) and Bi(NO3)3·5H2O (4850.7 mg, 10 mmol), dissolve in 2 mL of concentrated nitric acid, then add deionized water to dilute to 20 mL, and after magnetic stirring for a period of time, obtain a clear solution A. Weigh NH4VO3 (1638 mg, 14 mmol) and dissolve in 20 mL of 2 mol / L NaOH solution to obtain solution B. Under stirring, add solution B dropwise to solution A to form a yellow solution, then adjust the pH value of the mixed solution to 2 with 2 mol / L NaOH solution and continue magnetic stirring for 30 min after stabilization. Transfer the resulting mixture to a polytetrafluoroethylene reactor, place it in a forced air drying oven, and react at 180 ° C for 24 h; cool to room temperature and filter, rinse the filter residue three times with deionized water, and then wash it three times with anhydrous ethanol. Finally, the product was placed in a vacuum drying oven to dry, dried at 60°C for 6 hours, then ground and calcined at 500°C in a tubular furnace for 4 hours (heating rate of 5°C / min) to obtain a BiVO4 / FeVO4 composite material with a molar ratio of Bi(NO3)3·5H2O:Fe(NO3)3·9H2O=10:4 and a Fe(NO3)3·9H2O composite ratio of 40%.

[0034] (IV) BiVO4 / FeVO4 with a composite ratio of 50%

[0035] The preparation method is as follows:

[0036] Weigh Fe(NO3)3·9H2O (2020 mg, 5 mmol) and Bi(NO3)3·5H2O (4850.7 mg, 10 mmol), dissolve in 2 mL of concentrated nitric acid, then add deionized water to dilute to 20 mL, and after magnetic stirring for a period of time, obtain a clear solution A. Weigh NH4VO3 (1755 mg, 15 mmol) and dissolve in 20 mL of 2 mol / L NaOH solution to obtain solution B. Under stirring, add solution B dropwise to solution A to form a yellow solution, then adjust the pH value of the mixed solution to 2 with 2 mol / L NaOH solution and continue magnetic stirring for 30 min after stabilization. Transfer the resulting mixture to a polytetrafluoroethylene reactor, place it in a forced air drying oven, and react at 180 ° C for 24 h; cool to room temperature and filter, rinse the filter residue three times with deionized water, and then wash it three times with anhydrous ethanol. Finally, the product was placed in a vacuum drying oven to dry, dried at 60°C for 6 hours, then ground and calcined at 500°C in a tubular furnace for 4 hours (heating rate of 5°C / min) to obtain a BiVO4 / FeVO4 composite material with a molar ratio of Bi(NO3)3·5H2O:Fe(NO3)3·9H2O=10:5 and a Fe(NO3)3·9H2O composite ratio of 50%.

[0037] (V) BiVO4 / FeVO4 with a composite ratio of 60%

[0038] The preparation method is as follows:

[0039] Weigh Fe(NO3)3·9H2O (2424 mg, 6 mmol) and Bi(NO3)3·5H2O (4850.7 mg, 10 mmol), dissolve in 2 mL of concentrated nitric acid, then add deionized water to dilute to 20 mL, and after magnetic stirring for a period of time, obtain a clear solution A. Weigh NH4VO3 (1872 mg, 16 mmol) and dissolve in 20 mL of 2 mol / L NaOH solution to obtain solution B. Under stirring, add solution B dropwise to solution A to form a yellow solution, then adjust the pH value of the mixed solution to 2 with 2 mol / L NaOH solution and continue magnetic stirring for 30 min after stabilization. Transfer the resulting mixture to a polytetrafluoroethylene reactor, place it in a forced air drying oven, and react at 180 ° C for 24 h; cool to room temperature and filter, rinse the filter residue three times with deionized water, and then wash it three times with anhydrous ethanol. Finally, the product was placed in a vacuum drying oven to dry, dried at 60°C for 6 hours, then ground and calcined at 500°C in a tubular furnace for 4 hours (heating rate of 5°C / min) to obtain a BiVO4 / FeVO4 composite material with a molar ratio of Bi(NO3)3·5H2O:Fe(NO3)3·9H2O=10:6 and a Fe(NO3)3·9H2O composite ratio of 60%.

[0040] (VI) BiVO4 / FeVO4 with a composite ratio of 70%

[0041] The preparation method is as follows:

[0042] Weigh Fe(NO3)3·9H2O (2828 mg, 7 mmol) and Bi(NO3)3·5H2O (4850.7 mg, 10 mmol), dissolve in 2 mL of concentrated nitric acid, then add deionized water to dilute to 20 mL, and after magnetic stirring for a period of time, obtain a clear solution A. Weigh NH4VO3 (1989 mg, 17 mmol) and dissolve in 20 mL of 2 mol / L NaOH solution to obtain solution B. Under stirring, add solution B dropwise to solution A to form a yellow solution, then adjust the pH value of the mixed solution to 2 with 2 mol / L NaOH solution and continue magnetic stirring for 30 min after stabilization. Transfer the resulting mixture to a polytetrafluoroethylene reactor, place it in a forced air drying oven, and react at 180 ° C for 24 h; cool to room temperature and filter, rinse the filter residue three times with deionized water, and then wash it three times with anhydrous ethanol. Finally, the product was placed in a vacuum drying oven to dry, dried at 60°C for 6 hours, then ground and calcined at 500°C in a tubular furnace for 4 hours (heating rate of 5°C / min) to obtain a BiVO4 / FeVO4 composite material with a molar ratio of Bi(NO3)3·5H2O:Fe(NO3)3·9H2O=10:7 and a Fe(NO3)3·9H2O composite ratio of 70%.

[0043] (VII) Characterization

[0044] Figure 1 The XPS spectra of BiVO4, FeVO4 and BiVO4 / FeVO4 (composite ratio is 60%) are shown. The XPS spectrum shows that BiVO4 / FeVO4 contains Bi, V, O and Fe elements. The results confirm that the composite material synthesized by the present invention is composed of BiVO4 and FeVO4 nanoparticles.

[0045] Example 2 Effect of BiVO4 / FeVO4 Composite Materials on Catalytic Ultrasonic Removal of Tetracycline Solution (I) Effect of BiVO4 / FeVO4 Composite Materials with Different Composite Ratios on Ultrasonic Removal of Tetracycline

[0046] The method is as follows: 25 mg of BiVO4 / FeVO4 powder and 20 mL of 50 mg / L tetracycline (TET) solution are added to a conical flask to mix them, and then placed in an ultrasonic cleaner. The ultrasonic power is set to 500 W and ultrasonicated for 120 minutes under light-proof conditions. After the ultrasonication, the catalyst is filtered out with a filter head, and the absorbance is detected with an ultraviolet spectrophotometer. The data are recorded and saved, and the tetracycline removal rate is calculated according to formula (1).

[0047] Removal rate (%) = [(A0-A t ) / A0]×100%(1)

[0048] Where A0 is the initial absorbance of tetracycline, A t is the absorbance after the tetracycline solution was removed after each experiment.

[0049] In addition, the removal rate of TET solution is within its λ max = Calculated by absorbance at 350 nm.

[0050] The results are as follows Figure 2 As shown, when the composite ratio is 60%, the removal effect of the synthesized bismuth vanadate / iron vanadate catalyst is the best, and the removal rate can reach 71.13±2.06%. This is because the composite of bismuth vanadate and iron vanadate forms an S-type heterojunction, which can adjust its electronic structure and improve the disadvantage of high electron-hole recombination rate, thus improving the removal effect.

[0051] (II) Effect of BiVO4 / FeVO4 composite material and potassium persulfate on the removal of tetracycline solution by ultrasonic catalysis

[0052] The method is as follows: 25 mg of BiVO4 / FeVO4 powder (composite ratio of 60%) and 20 mL of 50 mg / L tetracycline (TET) solution are added to a conical flask to mix them, and then potassium persulfate is added to the conical flask, and the amount of potassium persulfate added is 5 mg, 15 mg, 20 mg, 30 mg, and 60 mg respectively; then it is placed in an ultrasonic cleaner, and the ultrasonic power is set to 500 W and ultrasonicated for 120 minutes under light-shielding conditions. After the ultrasonication ends, the catalyst is filtered out with a filter head, and the absorbance is detected with an ultraviolet spectrophotometer. The data are recorded and saved, and the removal rate of tetracycline is calculated according to formula (1).

[0053] The results are as follows Figure 3 As shown in the figure, with the increase of potassium persulfate concentration, the removal effect of tetracycline gradually increases. When the amount of potassium persulfate added is 60 mg, the removal rate of tetracycline can reach 94.80±1.09% in 120 minutes.

[0054] H + +S2O8 2- →HS2O8 - (2)

[0055] HS2O8 - →H + +SO4 2- +SO4 - (3)

[0056] H2O+SO4 - →H + + OH+SO4 2- (4)

[0057] As shown in the above formulas (2)-(4), the addition of K2S2O8 produces more active substances, which significantly improves its removal rate. The experimental results show that the synergistic ultrasonic catalytic removal of tetracycline solution by bismuth vanadate / iron vanadate composite material and potassium persulfate has the characteristics of high removal efficiency, short reaction time and low cost.

Claims

1. A bismuth vanadate / iron vanadate composite acoustic catalyst, characterized in that: The preparation method of the bismuth vanadate / iron vanadate composite acoustic catalyst comprises the following steps: taking Bi(NO3)3·5H2O and Fe(NO3)3·9H2O, adding nitric acid solution to dissolve, mixing evenly, slowly dropping NH4VO3 NaOH solution, adjusting the pH value of the solution, stirring evenly, transferring the mixed solution to a reactor for hydrothermal synthesis reaction, cooling to room temperature, filtering, washing, drying, and calcining at high temperature in a tubular furnace to obtain the bismuth vanadate / iron vanadate composite acoustic catalyst BiVO4 / FeVO4.

2. The bismuth vanadate / iron vanadate composite sonic catalyst according to claim 1, characterized in that: In molar ratio, Bi(NO3)3·5H2O:Fe(NO3)3·9H2O=10:(2~7); Bi(NO3)3·5H2O:NH4VO3=10:(12~17).

3. The bismuth vanadate / iron vanadate composite sonic catalyst according to claim 1, characterized in that: Adjust the solution pH to 1.5-2.

5.

4. The bismuth vanadate / iron vanadate composite sonic catalyst according to claim 1, characterized in that: The hydrothermal synthesis reaction is carried out at 175-185°C for 22-26 hours; the high-temperature calcination is carried out at a calcination temperature of 450-550°C, a calcination holding time of 4-5 hours, and a heating rate of 5°C / min.

5. Use of a bismuth vanadate / iron vanadate composite sonic catalyst as claimed in any one of claims 1 to 4 in catalytic removal of organic pollutants.

6. The use according to claim 5, characterized in that: The organic pollutant is tetracycline.

7. The use according to claim 6, characterized in that: The method is as follows: adding a bismuth vanadate / iron vanadate composite acoustic catalyst according to any one of claims 1 to 4 into wastewater containing tetracycline, and ultrasonicating.

8. The use according to claim 7, characterized in that: The addition amount of the bismuth vanadate / iron vanadate composite sonic catalyst is 1.0-1.5 mg / mL, the concentration of tetracycline is 40-60 mg / L, the ultrasonic power is 500 W, and the ultrasonic time is 100-150 min.

9. The use according to claim 8, characterized in that: Potassium persulfate was added at the same time.

10. The use according to claim 9, characterized in that: The amount of potassium persulfate added is 0.25-3.0 mg / mL.

Citation Information

Patent Citations

  • Preparation and application of CeVO4 / BiVO4 heterojunction with visible-light response

    CN108889294A

  • Preparation method and application of bismuth vanadate / copper tungstate composite acoustic catalyst

    CN117205938A

Cited By

  • Arsenic pollution remediation method based on piezoelectric catalysis in-situ self-Fenton reaction

    CN121494247A