Hydrocracking catalyst for high-yield low-freezing-point diesel distillate oil and preparation method of hydrocracking catalyst

By spraying low-concentration acid water and wet-mixed rolling into the dry powder mixture of hydrocracking catalyst, the preparation process is simplified, the complex and cost-effective preparation in the prior art is solved, and high-activity and low-coagulation diesel is achieved. Production and process simplification.

CN118988393APending Publication Date: 2024-11-22REZEL CATALYSTS CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411040719.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The preparation process of existing hydrocracking catalysts is complex and costly, and it is necessary to prepare binders first, resulting in cumbersome production processes and high costs, making it difficult to achieve industrial promotion.

Method used

Using the direct spraying of low-concentration acid water in the dry powder mixture, the hydrocracking catalyst carrier is made by wet mixing and rolling, the binder preparation steps are abandoned, the process flow is simplified, and the catalyst is improved by impregnating the active metal components. performance.

Benefits of technology

The production of high-activity and low-cooling point diesel is achieved, while reducing production costs and energy consumption, simplifying the process flow, and improving the specific surface area and performance of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a preparation method of a hydrocracking catalyst for high-yield low-freezing-point diesel distillate oil, which comprises the following steps: step 1, mixing a beta molecular sieve, amorphous silica-alumina, macroporous alumina, microporous alumina and an auxiliary agent, spraying a low-concentration nitric acid solution, uniformly wet-mixing, and grinding to obtain extrudable paste; extruding, drying and roasting to prepare a hydrocracking catalyst carrier; and 2, dipping the hydrocracking catalyst carrier obtained in the step 1 in a metal component solution containing hydrogenation activity, drying, and roasting to obtain the hydrocracking catalyst. According to the hydrocracking catalyst disclosed by the invention, the beta molecular sieve with proper silica-alumina ratio, large specific surface area, proper acidity, reasonable pore structure and low framework aluminum content is adopted as a cracking component; according to the method, the step of firstly preparing a binder in the preparation process of the hydrocracking catalyst carrier in the prior art is abandoned, and the low-concentration acid water is directly sprayed into the dry powder mixed material to obtain the catalyst carrier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrocracking catalysts, in particular to a hydrocracking catalyst for producing more low-condensation diesel fraction oil and a preparation method thereof. Background Art

[0002] As crude oil becomes heavier and inferior and environmental regulations become increasingly stringent, the realization of lightening of heavy oil, upgrading of inferior oil products and integration of refining and chemical industry have become hot topics in the field of petrochemical industry. Hydrocracking is a rapidly developing refining process that can increase the efficiency of oil refining and provide high-quality, low-sulfur intermediate distillate products. Ultra-low sulfur diesel produced by hydrocracking process is the most marketable product in most countries. Therefore, the development of high-activity and high-selectivity diesel-type hydrocracking catalysts is very urgent. At present, research institutions at home and abroad are constantly improving the performance of hydrocracking catalysts by synthesizing new materials, modifying molecular sieves, or optimizing catalyst preparation processes.

[0003] Patent CN104667966A uses modified β molecular sieve and amorphous silicon aluminum to provide acidic sites as cracking components. This patent uses β molecular sieve as an acidic component and adds amorphous silicon aluminum as a second cracking component, which can produce a good synergistic catalytic effect. While the activity of the hydrocracking catalyst is improved, it also has good properties such as selective ring opening of cycloalkanes, isomerization of chain alkanes, moderate hydrocracking of heavy fractions, and saturation of aromatics. While the hydrocracking catalyst is used to produce low-freezing point diesel in large quantities, it also takes into account the production of high-quality hydrogenated tail oil. However, the modified β molecular sieve in this patent first uses a hydrothermal method to treat the original molecular sieve powder, and then realizes the molecular sieve stripping template and selectively reduces the activation energy of the skeleton aluminum under the action of high-temperature dynamic hydrothermal steam, and needs to cooperate with the subsequent ammonium hexafluorosilicate modification process to stabilize the molecular sieve pore structure. The required β molecular sieve requires a complex modification process, which greatly increases the production cost and energy consumption of the catalyst. Moreover, the above catalyst preparation method requires first adding water and nitric acid to small-pore alumina to prepare a binder, and then kneading it with molecular sieves and large-pore alumina. The process is relatively complicated, and the binder is not easy to preserve. If it is not used in time, it is easy to cause material waste.

[0004] Patent CN107233927 discloses a method for preparing a medium oil type hydrocracking catalyst carrier, which uses fluorosilicic acid modified beta molecular sieve, amorphous silicon aluminum, macroporous alumina and small pore alumina to obtain a catalyst carrier with reasonable pore structure, large specific surface area, acidity and suitable acidity distribution. However, this method requires the use of fluorosilicic acid to acidify and modify the beta molecular sieve raw powder, and still needs to prepare the small pore alumina and nitric acid solution into a binder. The preparation process is complicated and the cost is high. On the other hand, the process of preparing the binder by reacting the small pore alumina with a large amount of nitric acid aqueous solution will cause the small pore alumina structure to collapse, so that the specific surface area of ​​the prepared catalyst carrier is greatly reduced.

[0005] Therefore, it is necessary to develop a simple and feasible method for preparing a high-yield diesel hydrocracking catalyst that avoids the preparation of a binder. The preparation method of the catalyst should have fewer steps and lower cost, and the production process should be easy to industrially implement and commercially promote. Summary of the invention

[0006] The technical purpose of the present invention is to provide a hydrocracking catalyst for producing more low-condensation diesel fraction oil and a preparation method thereof. The hydrocracking catalyst adopts a beta molecular sieve with a suitable silicon-aluminum ratio, a large specific surface area, suitable acidity, a reasonable pore structure and a low skeleton aluminum content as a cracking component; the method abandons the step of preparing a binder in the previous preparation process of the hydrocracking catalyst carrier, and the present invention directly sprays low-concentration acid water into the dry powder mixture to obtain the catalyst carrier.

[0007] In order to achieve the above technical objectives, the technical solution provided by the present invention is:

[0008] A method for preparing a hydrocracking catalyst for producing more low-condensate diesel distillate oil comprises the following steps:

[0009] Step 1: After mixing β molecular sieve, amorphous silicon aluminum, macroporous alumina, microporous alumina and additives, spraying low concentration nitric acid solution, wet mixing and rolling to prepare a hydrocracking catalyst carrier;

[0010] Step 2: The hydrocracking catalyst carrier obtained in step 1 is immersed in a solution containing a metal component having hydrogenation activity, and then dried and calcined to obtain a hydrocracking catalyst.

[0011] Furthermore, the mass concentration of the nitric acid solution is 2%-7%.

[0012] Furthermore, the spraying method is to mix the raw materials for 5-10 seconds first, and then spray for 5-10 seconds, with the spraying being staggered at this interval.

[0013] Furthermore, the beta molecular sieve, amorphous silica-alumina, macroporous alumina, microporous alumina and additive are added in a mass ratio of 5-10:70-80:20-25:30-45:1.

[0014] Furthermore, the molecular ratio of HNO3 to small pore alumina is 0.10-0.50.

[0015] Furthermore, the step 1, after wet mixing and rolling, also includes extrusion, drying and roasting.

[0016] Furthermore, the drying temperature is 70-150° C., and the drying time is 1-10 hours.

[0017] Furthermore, the calcination temperature is 300-600° C., and the calcination time is 1-5 hours.

[0018] Furthermore, the calcination temperature heating rate is greater than 160°C / min.

[0019] Furthermore, in step 2, the active metal component includes tungsten salt and / or nickel salt, the tungsten salt includes ammonium metatungstate, and the nickel salt includes nickel nitrate and nickel acetate.

[0020] Furthermore, in step 2, the immersion temperature is room temperature and the time is 2-5 hours.

[0021] Furthermore, in step 2, the drying temperature is 70-200°C.

[0022] Furthermore, in step 2, the calcination temperature is 300-600° C., and the calcination time is 1-6 hours.

[0023] The present invention also provides a hydrocracking catalyst, which comprises a carrier with cracking activity and a metal component with hydrogenation activity, wherein the carrier comprises beta molecular sieve, amorphous silica-alumina, macroporous alumina and microporous alumina; and the metal component with hydrogenation activity comprises WO3 and NiO.

[0024] Furthermore, the hydrocracking catalyst has a pore volume of >0.3 ml / g, a specific surface area of ​​>175 m2 / g, and an average crushing strength of >185 N / cm.

[0025] Furthermore, the β molecular sieve has a silicon-aluminum molecular ratio of 50-90, a pore volume of 0.25-0.45 ml / g, and a specific surface area of ​​450-650 m 2 / g, infrared total acid content 0.1-0.4mmol / g; the mass content of SiO2 in the amorphous silicon aluminum is 40%-60%, the pore volume is 0.4-1.5ml / g, and the specific surface area is 200-600m 2 / g; the macroporous alumina has a pore volume of 0.6-1.5 ml / g and a specific surface area of ​​200-600 m 2 / g; the pore volume of the small pore alumina is 0.25-0.75ml / g, and the specific surface area is 150-600m 2 / g.

[0026] Furthermore, the mass fraction of WO3 is 22-26%, and the mass fraction of NiO is 5.4-6.6%.

[0027] The present invention also provides a hydrocracking catalyst for producing more low-freezing-point diesel distillate oil and its application in producing low-freezing-point diesel by hydrocracking of heavy distillate oil.

[0028] The present invention has the following beneficial effects:

[0029] 1. The catalyst of the present invention is prepared by spraying acid water at intervals while mixing. Compared with the catalyst obtained by pouring acid water at one time, the catalyst has a larger specific surface area and higher diesel selectivity and yield under the same process conditions. It is further shown that the adhesive method of spraying acid water while mixing is more conducive to alleviating the degree of damage to the pore structure of alumina, which is beneficial to improving the specific surface area and catalytic performance of the catalyst.

[0030] 2. The present invention uses beta molecular sieve with a moderate silicon-aluminum ratio as the acidic component, combines amorphous silicon and aluminum to provide cracking sites, and cooperates with an appropriate content of hydrogenation metal sites to produce a synergistic catalytic effect, so that the hydrocracking catalyst has good cycloalkane selective ring opening, paraffin isomerization, heavy fraction moisture hydrocracking, aromatic saturation and heteroatom removal performance while improving its activity. The hydrocracking catalyst has high activity, can produce low-condensation point diesel in maximum quantity, and can also produce high-quality hydrogenated tail oil. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] In the description of the present invention, it should be noted that the directions or positional relationships indicated by "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. are based on the directions or positional relationships, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0033] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0034] A method for preparing a hydrocracking catalyst for producing more low-condensate diesel distillate oil comprises the following steps:

[0035] Step 1: After mixing β molecular sieve, amorphous silica-alumina, macroporous alumina, microporous alumina and additives, spray low concentration nitric acid solution, wet mix evenly and roll to a paste; and prepare a hydrocracking catalyst carrier through extrusion, drying and calcination.

[0036] Specifically, the mass concentration of the nitric acid solution is 2%-7%, preferably 3%-5%, ensuring that the molecular ratio of HNO3 to small-pore alumina is 0.10-0.50, preferably 0.25-0.35; the spraying method is to mix for 5-10 seconds, then spray for 5-10 seconds, and spray at this interval; the drying temperature is 70-150°C, preferably 110-120°C, the drying time is 1-10 hours, preferably 3-4 hours, ensuring that the water content on the surface of the extruded strip is less than 5%; the β molecular sieve, amorphous silicon aluminum, and macroporous oxide Aluminum, small pore alumina, and additives are added in a mass ratio of 5-10:70-80:20-25:30-45:1, and the additive is any one of sesbania powder, cellulose, clay, and vaseline, preferably sesbania powder, which has a certain viscosity and can improve the plasticity of the material, and has a certain lubricity and is convenient for extrusion; in step 1, the roasting temperature is 300-600°C, preferably 540-560°C, and the roasting time is 1-5 hours, preferably 2-4 hours; the roasting temperature heating rate is greater than 160°C / min.

[0037] The obtained hydrocracking catalyst carrier has a β molecular sieve weight content of 5-15%, preferably 6%-10%, based on the mass of the carrier; amorphous silicon aluminum content of 30-70%, preferably 45-55%; aluminum oxide content of 15%-65%, preferably 35%-50%; pore volume>0.50mL / g, specific surface area>260m 2 / g.

[0038] Step 2: The hydrocracking catalyst carrier obtained in step 1 is immersed in a solution containing a metal component having hydrogenation activity, and then dried and calcined to obtain a hydrocracking catalyst.

[0039] Specifically, in step 2, the active metal component includes tungsten salt and / or nickel salt, the tungsten salt includes ammonium metatungstate, and the nickel salt includes nickel nitrate and nickel acetate; in step 2, the impregnation temperature is room temperature, and the time is 2-5 hours, preferably 3-4 hours; in step 2, the drying temperature is 70-200°C, preferably 100-160°C; in step 2, the calcination temperature is 300-600°C, preferably 470-490°C, and the calcination time is 1-6 hours, preferably 2-4 hours.

[0040] The present invention also provides a hydrocracking catalyst, which comprises a carrier with cracking activity and a metal component with hydrogenation activity, wherein the carrier comprises β molecular sieve, amorphous silica-alumina, macroporous alumina and microporous alumina; the metal component with hydrogenation activity comprises WO3 and NiO; the hydrocracking catalyst has a pore volume of more than 0.3 ml / g and a specific surface area of ​​more than 175 m 2 / g, average crushing strength>185N / cm.

[0041] Specifically, the β molecular sieve has a silicon-aluminum molecular ratio of 50-90, preferably 60-80, a pore volume of 0.25-0.45 ml / g, preferably 0.3-0.4 ml / g, and a specific surface area of ​​450-650 m 2 / g, preferably 510-570m 2 / g, infrared total acid content 0.1-0.4mmol / g, preferably 0.2-0.3mmol / g; the mass content of SiO2 in the amorphous silicon aluminum is 40%-60%, preferably 45%-55%, the pore volume is 0.4-1.5ml / g, preferably 0.5-1.1ml / g, and the specific surface area is 200-600m 2 / g, preferably 220-500m 2 / g; the macroporous alumina has a pore volume of 0.6-1.5 ml / g and a specific surface area of ​​200-600 m 2 / g, preferably 230-500m 2 / g; the pore volume of the small-pore alumina is 0.25-0.75ml / g, preferably 0.40-0.50ml / g, and the specific surface area is 150-600m 2 / g, preferably 180-500m 2 / g; the WO3 mass fraction is 22-26%, and the NiO mass fraction is 5.4-6.6%.

[0042] The present invention also provides an application of a hydrocracking catalyst for producing more low-freezing-point diesel oil fractions in the hydrocracking of heavy distillate oil to produce low-freezing-point diesel oil. The hydrocracking conditions used are as follows: a single-stage process flow is adopted, the total reaction pressure is 12.0-20.0 MPa, the liquid hourly volume space velocity is 0.5-2.0 h -1 , hydrogen-oil volume ratio 1000:1-2000:1, reaction temperature 370-435°C.

[0043] The hydrocracking catalyst of the present invention can be used in the hydrocracking process of heavy distillate oil (VGO, CGO and DAO), wherein raw materials such as inferior diesel (coking diesel and catalytic diesel, etc.) can also be added.

[0044] Example 1

[0045] 28.2 g of β molecular sieve (dry basis 65%, silicon-aluminum ratio 60, pore volume 0.3 ml / g, specific surface area 510 m 2 / g), 230g amorphous silicon aluminum (dry basis 76%, SiO2 content 45%, pore volume 0.5ml / g, specific surface area 220m 2 / g), 70.3g macroporous alumina (dry basis 71%, pore volume 0.8ml / g, specific surface area 230m 2 / g), 139g small pore alumina (dry basis 64.5%, pore volume 0.4ml / g, specific surface area 180m 2 / g) and 3.33g of field sesbania powder were put into a kneader and dry mixed evenly. 16.6g of nitric acid (content 40g / 100ml) and 260g of water were prepared into a nitric acid aqueous solution with a mass fraction of 3.9%. The molar ratio of nitric acid to small pore alumina was 0.19. At room temperature, the mixture was first mixed for 5 seconds and then sprayed for 5 seconds at intervals. The mixture was added to the kneader, kneaded into a paste, and extruded into strips. The extruded strips were dried at 110°C for 4 hours and then calcined at 550°C for 4 hours to obtain the carrier RHC-S1. The properties are shown in Table 1. The carrier was impregnated with an impregnation solution containing tungsten and nickel at room temperature for 3 hours. The impregnated strips were dried at 120°C for 4 hours and calcined at 480°C for 4 hours to obtain the catalyst RHC-1. Its properties are shown in Table 1.

[0046] Example 2

[0047] 18.4 g of β molecular sieve (dry basis 100%, silicon-aluminum ratio 70, pore volume 0.4 ml / g, specific surface area 570 m 2 / g), 230g amorphous silicon aluminum (dry basis 76%, SiO2 content 50%, pore volume 0.8ml / g, specific surface area 300m 2 / g), 70.3g macroporous alumina (dry basis 71%, pore volume 0.9ml / g, specific surface area 300m 2 / g), 149g small pore alumina (dry basis 78%, pore volume 0.45ml / g, specific surface area 200m 2 / g) and 3.33g of field sesbania powder were put into a kneader and dry mixed evenly. 16.6g of nitric acid (content 40g / 100ml) and 2000g of water were prepared into a nitric acid aqueous solution with a mass fraction of 5.0%. The molar ratio of nitric acid to small pore alumina was 0.18. At room temperature, they were mixed for 10 seconds and then sprayed at intervals of 10 seconds before being added to the kneader, kneaded into a paste, and extruded. The extruded strips were dried at 115°C for 3 hours, and then calcined at 540°C for 2 hours to obtain the carrier RHC-S2. The properties are shown in Table 1. The carrier was impregnated with an impregnation solution containing tungsten and nickel at room temperature for 4 hours. The impregnated strips were dried at 100°C for 4 hours and calcined at 470°C for 2 hours to obtain the catalyst RHC-2. Its properties are shown in Table 1.

[0048] Example 3

[0049] 18.8 g of β molecular sieve (dry basis 97%, silicon-aluminum ratio 50, pore volume 0.25 ml / g, specific surface area 450 m 2 / g), 230g amorphous silicon aluminum (dry basis 76%, SiO 2 Content 40%, pore volume 0.4ml / g, specific surface area 200m 2 / g), 70.3g macroporous alumina (dry basis 71%, pore volume 0.6ml / g, specific surface area 200m 2 / g), 129g small pore alumina (dry basis 78%, pore volume 0.25ml / g, specific surface area 250m 2 / g) and 3.33g of field sesbania powder are put into a kneader and dry mixed evenly. 16.6g of nitric acid (content 40g / 100ml) and 290g of water are prepared into a nitric acid aqueous solution with a mass fraction of 3.5%. The molar ratio of nitric acid to small pore alumina is 0.21. At room temperature, mix for 6 seconds and then spray for 6 seconds at intervals. Add it to the kneader, knead it into a paste, and extrude it into strips. The extruded strips are dried at 70°C for 10 hours, and then calcined at 300°C for 5 hours to obtain the carrier RHC-S3. The properties are shown in Table 1. The carrier is impregnated with an impregnation solution containing tungsten and nickel at room temperature for 3 hours. The impregnated strips are dried at 70°C for 4 hours and calcined at 300°C for 6 hours to obtain the catalyst RHC-3. Its properties are shown in Table 1.

[0050] Example 4

[0051] 18.4 g of β molecular sieve (dry basis 100%, silicon-aluminum ratio 90, pore volume 0.45 ml / g, specific surface area 650 m 2 / g), 269g amorphous silicon aluminum (dry basis 65%, SiO2 content 60%, pore volume 1.5ml / g, specific surface area 600m 2 / g), 80.5g macroporous alumina (dry basis 62%, pore volume 1.5ml / g, specific surface area 600m 2 / g), 119g small pore alumina (dry basis 68%, pore volume 0.75ml / g, specific surface area 600m 2 / g) and 3.33g of field sesbania powder are put into a kneader and dry mixed evenly. 16.6g of nitric acid (content 40g / 100ml) and 300g of water are prepared into a nitric acid aqueous solution with a mass fraction of 3.4%. The molar ratio of nitric acid to small pore alumina is 0.23. At room temperature, mix for 7 seconds and then spray for 7 seconds at staggered intervals before adding it to the kneader, kneading into a paste and extruding strips. The extruded strips are dried at 150°C for 1 hour and then calcined at 600°C for 1 hour to obtain the carrier RHC-S4. The properties are shown in Table 1. The carrier is impregnated with an impregnation solution containing tungsten and nickel at room temperature for 4 hours. The impregnated strips are dried at 200°C for 3 hours and calcined at 600°C for 1 hour to obtain the catalyst RHC-5. Its properties are shown in Table 1

[0052] Example 5

[0053] 18.4 g of β molecular sieve (dry basis 100%, silicon-aluminum ratio 80, pore volume 0.3 ml / g, specific surface area 510 m 2 / g), 269g amorphous silicon aluminum (dry basis 65%, SiO2 content 55%, pore volume 1.1ml / g, specific surface area 500m 2 / g), 73.4g macroporous alumina (dry basis 68%, pore volume 1.0ml / g, specific surface area 500m 2 / g), 109g small pore alumina (dry basis 68%, pore volume 0.5ml / g, specific surface area 500m 2 / g) and 3.33g of field sesbania powder were put into a kneader and dry mixed evenly. 16.6g of nitric acid (content 40g / 100ml) and 210g of water were prepared into a nitric acid aqueous solution with a mass fraction of 4.8%. The molar ratio of nitric acid to small pore alumina was 0.25. At room temperature, the mixture was first mixed for 8 seconds and then sprayed for 8 seconds at intervals. The mixture was added to the kneader, kneaded into a paste, and extruded into strips. The extruded strips were dried at 120°C for 4 hours, and then calcined at 560°C for 4 hours to obtain the carrier RHC-S5. The properties are shown in Table 1. The carrier was impregnated with an impregnation solution containing tungsten and nickel at room temperature for 3 hours. The impregnated strips were dried at 160°C for 4 hours and calcined at 490°C for 4 hours to obtain the catalyst RHC-5. Its properties are shown in Table 1.

[0054] Comparative Example 1

[0055] This comparative example adopts a mixing method of pouring acid water at one time. 18.4g of β molecular sieve (dry basis 100%, silicon-aluminum ratio 75, pore volume 0.35ml / g, specific surface area 540m 2 / g), 230g amorphous silicon aluminum (dry basis 76%, SiO2 content 50%, pore volume 0.9ml / g, specific surface area 300m 2 / g), 70.3g macroporous alumina (dry basis 71%, pore volume 1.0ml / g, specific surface area 300m 2 / g), 99g small pore alumina (dry basis 78%, pore volume 0.4ml / g, specific surface area 200m 2 / g) and 3.33g of field sesbania powder are put into a kneader and dry mixed evenly. 16.6g of nitric acid (content 40g / 100ml) and 230g of water are prepared into a nitric acid aqueous solution with a mass fraction of 4.4%. The molar ratio of nitric acid to small pore alumina is 0.27. Pour them into the kneader at room temperature at one time, knead them into a paste, and extrude them into strips. The extruded strips are dried at 120°C for 3 hours, and then calcined at 550°C for 4 hours to obtain the carrier RHC-S6. The properties are shown in Table 1. The carrier is impregnated with an impregnation solution containing tungsten and nickel at room temperature for 4 hours. The impregnated strips are dried at 100°C for 4 hours and calcined at 480°C for 4 hours to obtain the catalyst RHC-6. Its properties are shown in Table 1.

[0056] Comparative Example 2

[0057] Comparative Example: A catalyst carrier was prepared by using a binder and then impregnated to prepare a hydrocracking catalyst. 18.4 g of β molecular sieve (dry basis 100%, silicon-aluminum ratio 70, pore volume 0.4 ml / g, specific surface area 570 m 2 / g), 230g amorphous silicon aluminum (dry basis 76%, SiO2 content 50%, pore volume 0.8ml / g, specific surface area 300m 2 / g), 70.3g macroporous alumina (dry basis 71%, pore volume 0.9ml / g, specific surface area 300m 2 / g), 3.33g of sesbania powder were put into a kneader and dry-mixed evenly, 346g of binder (109g of small-pore alumina (dry basis 78%, pore volume 0.45ml / g, specific surface area 200m 2 / g), 16.6g nitric acid (content 40g / 100ml) and 190g water, the molar ratio of nitric acid to small pore alumina is 0.25) are added to a kneader, kneaded into a paste, and extruded. The extruded strips are dried at 115°C for 3 hours, and then calcined at 540°C for 2 hours to obtain the carrier RHC-S7. The properties are shown in Table 1. The carrier is impregnated with an impregnation solution containing tungsten and nickel at room temperature for 4 hours. The impregnated strips are dried at 100°C for 4 hours and calcined at 470°C for 2 hours to obtain the catalyst RHC-7. Its properties are shown in Table 1.

[0058] Table 1 Physicochemical properties of catalyst carrier and catalyst

[0059]

[0060] The catalysts prepared in Examples 1-6 and Comparative Example 1 were evaluated in a fixed bed hydrogenation test device under the following conditions: total reaction pressure of 15.0 MPa, hydrogen to oil volume ratio of 1500, and volume space velocity of 0.9 h -1 , using vacuum distillate oil (VGO) as the feedstock oil, the properties of the feedstock oil are listed in Table 2. Catalysts RHC-1 to RHC-7 were evaluated under the same process conditions, and the evaluation results are listed in Table 3.

[0061] Table 2 Raw oil properties

[0062] Crude oil VGO-1 VGO-2 Density 20℃, g / cm3 0.9054 0.9118 Distillation range / ℃ IBP / 10% 30 / 361 314 / 387 30% / 50% 392 / 414 415 / 439 70% / 90% 443 / 483 476 / 521 95% / EBP 510 / 552 540 / 552 Pour point, ℃ 34 32 Sulfur, wt% 2.05 1.75 Nitrogen, μg / g 1176 1237 Carbon, wt% 85.31 95.34 Hydrogen, wt% 12.61 12.66 BMCI value 44.08 44.32

[0063] Table 3 Performance evaluation conditions and results

[0064]

[0065]

[0066] It can be seen from the evaluation results in Table 3 that the specific surface area of ​​the catalyst of the present invention is much larger than that of the catalyst obtained by preparing a binder. Under the same process conditions, the diesel selectivity, yield and product quality are better than those of the reference catalyst obtained by first preparing a binder and then preparing a carrier. At the same time, the preparation process of the catalyst of the present invention is greatly simplified compared with the reference catalyst. On the other hand, the catalyst prepared by spraying acid water while mixing has a larger specific surface area than the catalyst obtained by pouring acid water at one time, and has higher diesel selectivity and yield under the same process conditions. This also further shows that the adhesive method of spraying acid water while mixing is more conducive to alleviating the degree of damage to the pore structure of alumina, and is conducive to improving the specific surface area and catalytic performance of the catalyst.

[0067] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0068] The above specific implementation methods are detailed descriptions of the present invention. It cannot be determined that the specific implementation methods of the present invention are limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions and substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.

Claims

1. A method for preparing a hydrocracking catalyst for producing more low-condensation diesel distillate oil, characterized in that: The steps include: Step 1: After mixing β molecular sieve, amorphous silicon aluminum, macroporous alumina, microporous alumina and additives, spraying low concentration nitric acid solution, wet mixing and rolling to prepare a hydrocracking catalyst carrier; Step 2: The hydrocracking catalyst carrier obtained in step 1 is immersed in a solution containing a metal component having hydrogenation activity, and then dried and calcined to obtain a hydrocracking catalyst.

2. The method for preparing a hydrocracking catalyst for producing high-yield low-condensate diesel distillate according to claim 1, characterized in that: The mass concentration of the nitric acid solution is 2%-7%.

3. The method for preparing a hydrocracking catalyst for producing high-yield low-condensate diesel distillate according to claim 1, characterized in that: The spraying method is to mix the raw materials for 5-10 seconds first, and then spray for 5-10 seconds, with the spraying being staggered at this interval.

4. The method for preparing a hydrocracking catalyst for producing high-yield low-condensate diesel distillate according to claim 1, characterized in that: The beta molecular sieve, amorphous silicon aluminum, macroporous alumina, microporous alumina and auxiliary agent are added in a mass ratio of 5-10:70-80:20-25:30-45:

1.

5. The method for preparing a hydrocracking catalyst for producing high-yield low-condensate diesel distillate according to claim 1, characterized in that: The molecular ratio of HNO3 to small pore alumina is 0.10-0.

50.

6. The method for preparing a hydrocracking catalyst for producing high-yield low-condensate diesel distillate according to claim 1, characterized in that: The step 1, after wet mixing and rolling, also includes extrusion, drying and roasting.

7. The method for preparing a hydrocracking catalyst for producing high-yield low-condensate diesel distillate according to claim 6, characterized in that: The drying temperature is 70-150° C., and the drying time is 1-10 hours.

8. The method for preparing a hydrocracking catalyst for producing high-yield low-condensate diesel distillate according to claim 6, characterized in that: The calcination temperature is 300-600° C., and the calcination time is 1-5 hours.

9. The method for preparing a hydrocracking catalyst for producing high-yield low-condensate diesel distillate according to claim 6, characterized in that: The calcination temperature heating rate is greater than 160°C / min.

10. The method for preparing a hydrocracking catalyst for producing high-yield low-condensate diesel fraction according to claim 1, characterized in that: In step 2, the active metal component includes tungsten salt and / or nickel salt, the tungsten salt includes ammonium metatungstate, and the nickel salt includes nickel nitrate and nickel acetate.

11. The method for preparing a hydrocracking catalyst for producing high-yield low-condensate diesel fraction according to claim 1, characterized in that: In step 2, the immersion temperature is room temperature and the time is 2-5 hours.

12. The method for preparing a hydrocracking catalyst for producing high-yield low-condensate diesel fraction according to claim 1, characterized in that: In step 2, the drying temperature is 70-200°C.

13. The method for preparing a hydrocracking catalyst for producing high-yield low-condensate diesel distillate according to claim 1, characterized in that: In step 2, the calcination temperature is 300-600° C., and the calcination time is 1-6 hours.

14. A hydrocracking catalyst is obtained by using the method for preparing a hydrocracking catalyst for producing a high yield of low-condensation diesel fraction according to any one of claims 1 to 13, characterized in that: The hydrocracking catalyst comprises a carrier with cracking activity and a metal component with hydrogenation activity, wherein the carrier comprises beta molecular sieve, amorphous silica-alumina, macroporous alumina and microporous alumina; the metal component with hydrogenation activity comprises WO3 and NiO.

15. A hydrocracking catalyst according to claim 14, characterized in that: The hydrocracking catalyst has a pore volume of >0.3 ml / g and a specific surface area of ​​>175 m 2 / g, average crushing strength>185N / cm.

16. A hydrocracking catalyst according to claim 14, characterized in that: The beta molecular sieve has a silicon-aluminum molecular ratio of 50-90, a pore volume of 0.25-0.45 ml / g, and a specific surface area of ​​450-650 m 2 / g, infrared total acid content 0.1-0.4mmol / g; the mass content of SiO2 in the amorphous silicon aluminum is 40%-60%, the pore volume is 0.4-1.5ml / g, and the specific surface area is 200-600m 2 / g; the macroporous alumina has a pore volume of 0.6-1.5 ml / g and a specific surface area of ​​200-600 m 2 / g; the pore volume of the small pore alumina is 0.25-0.75ml / g, and the specific surface area is 150-600m 2 / g.

17. A hydrocracking catalyst according to claim 14, characterized in that: The mass fraction of WO3 is 22-26%, and the mass fraction of NiO is 5.4-6.6%.

18. Use of a hydrocracking catalyst capable of producing more low-freezing-point diesel distillate oil as claimed in claim 14 in the production of low-freezing-point diesel by hydrocracking of heavy distillate oil.

Citation Information

Patent Citations

  • Preparation method for MFI / MOR composite zeolite molecular sieve catalyst without binder

    CN102188993A

  • Preparation method of hydrogenation catalyst

    CN102451743A

  • Hydrocracking catalyst carrier containing beta molecular sieve and preparation method thereof

    CN103100427A

  • A hydrocracking catalyst carrier and a preparing method thereof

    CN104667957A

  • A hydrocracking catalyst and a preparing method thereof

    CN104667958A