Casting mechanism for medical magnesium alloy

By designing a medical magnesium alloy casting mechanism containing filters and inert gas introduction valves, the problems of inclusion and gas mixing and composition segregation in magnesium alloy casting are solved, and safe and efficient preparation of magnesium alloy materials are achieved, suitable for small diameters and long sizes Product production and reduce operational risks.

CN118989245APending Publication Date: 2024-11-22SHANGHAI BAIYUE MEDICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411403044.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing medical metal materials are difficult to remove in the human body, leading to risks such as inflammatory reactions, and long-sized magnesium alloys are prone to inclusions and gases when casting, resulting in component segregation and safety hazards.

Method used

A casting mechanism for medical magnesium alloy is designed, including a cover body, a cast-molded pipe body, a filter clamp seat, a connecting pipe body and a bottom plate, a filter and an inert gas introduction valve are provided, and a molten metal surface grade sensor and a pressure reducing pump are used. Control the inflow and solidification of molten metals to avoid mixing inclusions and gases, and ensure uniformity of components.

Benefits of technology

It realizes efficient and safe preparation of small diameter and long-size medical magnesium alloy materials, avoids the risks of component segregation and leakage, is suitable for existing smelting furnace installation, and reduces space requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989245A_ABST
    Figure CN118989245A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of production devices of biomedical metal materials, and relates to a casting mechanism of a medical magnesium alloy. The casting mechanism comprises a cover body, a casting mold pipe body, a filter clamping seat, a connecting pipe body and a bottom plate which are sequentially connected from top to bottom, a filter is arranged in the filter clamping seat, and a molten metal surface grade sensor, an inert gas leading-in valve and a pressure reduction pump connecting part are arranged on the cover body. Through the arrangement of the filter in the casting mechanism, inclusion and gas mixing and composition segregation can be avoided, and therefore a medical magnesium alloy casting material is produced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of production equipment for biomedical metal materials and relates to a casting mechanism for medical magnesium alloys. Background Art

[0002] At present, the main medical metal materials widely used in clinical practice include stainless steel, titanium alloy, cobalt-chromium alloy, etc. These materials have excellent corrosion resistance. However, this property also means that metal materials will remain in the human body permanently. For secondary surgeries aimed at removing medical devices after healing and for medical devices that are difficult to remove, there are many risks such as late postoperative inflammatory reactions.

[0003] In order to solve the risks of existing implantable medical devices, materials that can be degraded and absorbed in the human body have received widespread attention. Among these materials, experts have great expectations for magnesium and magnesium alloys (hereinafter referred to as magnesium alloys) for the following reasons: (1) Magnesium is a major element necessary for the human body, is not prone to poisoning, and is relatively safe in the human body; (2) Compared with non-degradable medical metals, the Young's modulus of magnesium and magnesium alloys is closest to that of human bones, which can effectively reduce stress shielding; (3) Compared with polylactic acid materials, magnesium alloys have better mechanical properties. Compared with traditional magnesium alloy uses, the size of component materials required for implantable medical devices is extremely small. For this reason, the shape of the casting material is also preferably small in diameter. Due to the relationship between product yield, a longer length is preferred. However, for extremely long casting molds, inclusions and gases are easily mixed and solidified during casting. In addition, in order to avoid the above problems, once the time of maintaining the molten metal state after casting is extended, component segregation will occur. The use of semi-continuous casting equipment makes it difficult to mix inclusions or gases, and can avoid the occurrence of component segregation, thereby producing longer-sized casting materials. However, in order to achieve this goal, the scale of the casting mechanism is large, and it is difficult to subsequently install it on an existing smelting furnace or holding furnace. In addition, the range of suitable casting conditions for semi-continuous casting becomes narrower as the caliber becomes smaller. Inappropriate production conditions can cause leakage of molten metal, bringing difficulties to production, including dangers such as water vaporization explosion and fire. Summary of the invention

[0004] In view of the shortcomings of the prior art described above, the purpose of the present invention is to provide a casting mechanism for medical magnesium alloys. By using the casting mechanism of the present invention, the mixing of inclusions and gases and the occurrence of component segregation can be avoided, thereby efficiently and safely preparing medical magnesium alloy materials to solve the problems in the prior art.

[0005] To achieve the above-mentioned purpose and other related purposes, the present invention provides a casting mechanism for medical magnesium alloy on the one hand, comprising a cover body, a casting mold tube body, a filter clamp seat, a connecting tube body and a bottom plate connected in sequence from top to bottom, a filter is provided in the filter clamp seat, and a molten metal surface level sensor, an inert gas inlet valve and a pressure reducing pump connection part are respectively provided on the cover body.

[0006] In some embodiments of the present invention, the inner diameter of the casting mold tube body is 30±5 mm; the wall thickness of the casting mold tube body is 2±1 mm; and the length of the casting mold tube body is 500 to 1500 mm.

[0007] In some embodiments of the present invention, an upper flange is provided on the casting mold tube body, and the cover body and the casting mold tube body are connected via the upper flange.

[0008] In some embodiments of the present invention, a lower flange is provided on the casting mold tube body, and the filter clamp seat and the casting mold tube body are connected via the lower flange.

[0009] In some embodiments of the present invention, the filter holder includes an opening portion, the filter is disposed in the opening portion, and the surface area of ​​the bottom plate is greater than the surface area of ​​the opening portion.

[0010] In some embodiments of the present invention, the filter is made of a material that does not react with the magnesium alloy molten metal.

[0011] In some embodiments of the present invention, the pore size of the filter gradually decreases from an end close to the connecting tube body to an end close to the casting mold tube body.

[0012] In some embodiments of the present invention, the distance between the filter holder and the bottom plate is 15±10 mm.

[0013] In some embodiments of the present invention, the molten metal surface level sensor, the inert gas introduction valve and the pressure reducing pump connection part are respectively connected to the casting mold tube body.

[0014] The present invention also provides a method for preparing a casting material using the casting mechanism of the medical magnesium alloy as described above, comprising the following steps:

[0015] 1) Introducing inert gas into the mold tube body through the inert gas introduction valve;

[0016] 2) preheating the casting mold tube and sinking the casting mechanism into the molten metal;

[0017] 3) Turn on the pressure reducing pump connected to the pressure reducing pump connection part to suck the molten metal into the mold tube;

[0018] 4) After confirming that the molten metal has risen to a certain height from a part of the filter using a molten metal surface level sensor, the pressure reducing pump is turned off;

[0019] 5) removing the casting mechanism from the molten metal and cooling the casting mold tube body to solidify the molten metal in the casting mold tube body;

[0020] 6) The solidified molten metal is taken out to obtain a casting material.

[0021] The beneficial effects of the technical solution of the present invention are:

[0022] By utilizing the setting of the filter in the casting mechanism of the present invention, the occurrence of inclusions, gas mixing and component segregation can be avoided, thereby producing a casting material of a medical magnesium alloy, preferably a casting material with a small diameter and a longer size. In addition, the casting mechanism of the present invention can be subsequently installed on the existing smelting casting mechanism. In addition, since the molten metal is covered by the steel pipe, the molten metal liquid will not leak under inappropriate casting conditions like a semi-continuous casting casting mechanism, thereby causing water vaporization explosion, fire and other dangers. Compared with the traditional magnesium alloy casting casting mechanism, the operation of the casting mechanism does not require a wide space. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic structural diagram showing the casting mechanism of the medical magnesium alloy of the present invention.

[0024] Figure 2 Shown is a schematic structural diagram of the casting mechanism used in Comparative Examples 1 and 2 of the present invention.

[0025] Figure 3 Shown is a schematic structural diagram of the casting mechanism used in Comparative Example 3 of the present invention.

[0026] Component numbers in the figure

[0027] 1 Cover

[0028] 2 cast tube body

[0029] 21 Upper flange

[0030] 22 Lower flange

[0031] 3 Filter holder

[0032] 31 Opening

[0033] 4 Connecting pipe

[0034] 5 Bottom plate

[0035] 6 Filters

[0036] 7 Molten Metal Surface Level Sensor

[0037] 8 Inert gas inlet valve

[0038] 9 Pressure reducing pump connection DETAILED DESCRIPTION

[0039] In the description of the present invention, it should be noted that the structures, proportions, sizes, etc. illustrated in the drawings of the present specification are only used to match the contents disclosed in the specification for people familiar with the technology to understand and read, and are not used to limit the limiting conditions that the present invention can be implemented, so they have no technical substantive significance. Any modification of the structure, change of the proportion relationship or adjustment of the size, without affecting the effects that the present invention can produce and the purposes that can be achieved, should still fall within the scope of the technical content disclosed by the present invention. At the same time, the directions or positional relationships indicated by the terms "center", "longitudinal", "lateral", "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc. are based on the directions or positional relationships shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0040] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0041] Furthermore, in the description of the present invention, unless otherwise specified, “plurality” means two or more.

[0042] like Figure 1 An embodiment of the present invention relates to a casting mechanism for a medical magnesium alloy, the casting mechanism comprising a cover body 1, a casting mold tube body 2, a filter clamp seat 3, a connecting tube body 4 and a bottom plate 5 which are sequentially connected from top to bottom, a filter 6 is provided in the filter clamp seat 3, and a molten metal surface level sensor 7, an inert gas inlet valve 8 and a pressure reducing pump connecting part 9 are respectively provided on the cover body 1.

[0043] In the casting mechanism of the medical magnesium alloy provided in the embodiment of the present invention, the cover body 1 is used to cover the mold tube body 2. The cover body 1 can be used to adjust the length of the casting material. The cover body 1 is connected to the pressure reducing pump via the pressure reducing pump connection part 9. The pressure reducing pump is used to reduce pressure, and the molten metal is gradually sucked into the mold tube body 2. Through the inserted molten metal surface level sensor 7 (such as a laser rangefinder or a contact rangefinder), the pressure reduction is stopped when any molten metal surface height that needs to be adjusted is reached.

[0044] In the casting mechanism of the medical magnesium alloy provided in the embodiment of the present invention, the mold tube body 2 is used for the casting mold. In some embodiments, the mold tube body 2 is a long steel tube, and the long steel tube is an integrated tube. The inner diameter of the mold tube body 2 is the outer diameter of the casting material produced, and its inner diameter can be arbitrarily changed according to the outer diameter of the casting material to be produced. In some embodiments, the inner diameter of the mold tube body 2 is 30±5mm; the wall thickness of the mold tube body 2 is 2±1mm according to the balance between thermal deformation and heat conduction; the length of the mold tube body 2 is 500-1500mm.

[0045] In the casting mechanism of the medical magnesium alloy provided in the embodiment of the present invention, Figure 1 The mold tube body 2 is provided with an upper flange 21 , and the cover body 1 and the mold tube body 2 are connected via the upper flange 21 .

[0046] In the casting mechanism of the medical magnesium alloy provided in the embodiment of the present invention, Figure 1 The casting mold tube body 2 is provided with a lower flange 22 , and the filter clamp seat 3 and the casting mold tube body 2 are connected via the lower flange 22 .

[0047] In the casting mechanism of the medical magnesium alloy provided in the embodiment of the present invention, Figure 1 The filter holder 3 includes an opening 31, and the filter 6 is disposed in the opening 31. In some embodiments, the filter holder 3 is composed of two flanges, and there is a gap between the two flanges for installing the filter 6, that is, the opening 31.

[0048] In the casting mechanism of the medical magnesium alloy provided in the embodiment of the present invention, the filter 6 has the function of preventing the molten metal from flowing back. Specifications of the filter 6: A material that does not react with the molten metal of the magnesium alloy should be selected, that is, the material of the filter 6 is a material that does not react with the molten metal of the magnesium alloy. Items related to filtering performance and life, such as pore size and thickness, will change according to the alloy composition, cleanliness of raw materials, smelting conditions, etc., and are also related to the inclusion content in the molten metal and the viscosity of the molten metal. Therefore, appropriate selection should be made in combination with specific conditions. Optionally, the pore size of the filter 6 gradually decreases from one end close to the connecting tube body 4 to one end close to the casting mold tube body 2. In some embodiments, the filter 6 can be, for example, a filter made of magnesium oxide, and the pore size of the filter 6 is 100 to 1000 μm and the thickness is 30 to 50 mm.

[0049] In the casting mechanism of the medical magnesium alloy provided in the embodiment of the present invention, Figure 1 , the bottom of the filter holder 3 is connected to the bottom plate 5 via the connecting tube body 4. The surface area of ​​the bottom plate 5 should be larger than the surface area of ​​the opening 31 of the filter holder 3. In some embodiments, the bottom plate 5 is arranged directly below the opening 31 of the filter 6. The bottom plate 5 can be used to avoid sucking in dirty molten metal with many inclusions near the bottom of the furnace. In addition, it can also avoid the oxide film on the surface of the molten metal adhering to the filter 6 when the casting mechanism sinks into the molten metal, thereby causing the filter 6 to be blocked. In some embodiments, the connecting tube body 4 can be, for example, a steel rod.

[0050] In the casting mechanism of the medical magnesium alloy provided in the embodiment of the present invention, the distance between the filter clamp seat 3 and the bottom plate 5 is 15±10 mm, that is, the height of the connecting tube body 4 .

[0051] In the casting mechanism of medical magnesium alloy provided in an embodiment of the present invention, a molten metal surface level sensor 7, an inert gas inlet valve 8 and a pressure reducing pump connecting part 9 are respectively provided on the cover body 1, and the molten metal surface level sensor 7, the inert gas inlet valve 8 and the pressure reducing pump connecting part 9 are respectively connected to the casting mold tube body 2.

[0052] In the casting structure of the medical magnesium alloy provided in the embodiment of the present invention, the material of the parts in contact with the molten metal should be stainless steel or steel treated with aluminum immersion.

[0053] In the casting mechanism of the medical magnesium alloy provided in the embodiment of the present invention, each connection point among the cover body 1, the casting mold tube body 2, the filter clamp seat 3, the connecting tube body 4 and the bottom plate 5 is an airtight structure through metal contact.

[0054] The working process of the casting mechanism of the medical magnesium alloy provided by the present invention is as follows:

[0055] Casting operation 1: Before immersing the casting mechanism in the molten metal, an inert gas is introduced so that the inert gas fills the inside of the mold tube 2. Once the atmosphere (oxygen, nitrogen, etc.) remains inside the mold tube 2, the atmosphere will react with the magnesium molten metal and become a cause of pollution, so this is a necessary operation.

[0056] Casting operation 2: While continuously introducing a certain amount of inert gas, slowly sink the casting structure into the molten metal. It is better if the casting structure can be preheated using an electric furnace. This operation can reduce the risk of unexpected molten metal temperature drop, water vaporization explosion, etc.

[0057] Casting operation 3: After the casting mechanism is sunk to an arbitrary height, the vacuum pump connected to the vacuum pump connection part 9 is operated to suck the molten metal into the mold tube body 2.

[0058] Casting operation 4: After confirming that the molten metal has risen to a specified height using the molten metal surface level sensor 7, the pressure reducing pump is turned off. At this time, if the aperture size of the filter 6 is appropriate, the molten metal will not flow back and the oil level can be maintained.

[0059] Casting operation 5: The casting structure is fished out from the molten metal and air-cooled. Alternatively, the mold tube body 2 is directly or indirectly water-cooled to solidify the molten metal in the steel tube.

[0060] Type of release agent: A release agent may also be used as required. A type that will not fall off due to thermal shock and be mixed into the molten metal should be selected. More preferably, a water-soluble release agent is applied to the inside of the mold tube 2 using a brush. Once there is residual water inside the mold tube 2, there is a high risk of water vaporization explosion when it comes into contact with the molten metal, so sufficient preheating and drying treatment must be performed to completely evaporate the water.

[0061] The present invention also provides a method for preparing a casting material of a casting mechanism of a medical magnesium alloy, characterized in that it comprises the following steps:

[0062] 1) Introducing inert gas into the mold tube body 2 through the inert gas introduction valve 8;

[0063] 2) preheating the mold tube 2 and sinking the casting mechanism into the molten metal;

[0064] 3) Turn on the pressure reducing pump connected to the pressure reducing pump connection part 9 to suck the molten metal into the mold tube body 2;

[0065] 4) After confirming that the molten metal has risen to a certain height from a part of the filter 6 using the molten metal surface level sensor 7, the pressure reducing pump is turned off;

[0066] 5) taking the casting mechanism out of the molten metal and cooling the mold tube body 2 so that the molten metal in the mold tube body 2 solidifies;

[0067] 6) The solidified molten metal is taken out to obtain a casting material.

[0068] Example 1

[0069] Use as Figure 1 The casting mechanism of the structure shown is used to prepare small-diameter long tube casting materials.

[0070] Regarding the type of magnesium alloy, Mg-2wt%Zn alloy was prepared and produced.

[0071] The mold tube body 2 is a long steel tube with flanges at both ends, with an inner diameter of 30 mm, a wall thickness of 1 mm, and a length of 1500 mm.

[0072] The lower flange 22 is connected to the filter holder 3. The filter holder 3 is composed of two flanges, and there is a gap, that is, an opening 31, between the two flanges, in which the filter 6 can be installed.

[0073] Specifications of filter 6: A filter 6 made of magnesium oxide is used, and the pore size of the filter 6 gradually decreases from bottom to top.

[0074] The bottom of the filter holder 3 is connected to the bottom plate 5 via a steel rod. The area of ​​the bottom plate 5 is larger than the opening 31 of the filter holder 3. The distance between the filter holder 3 and the bottom plate 5 is 10 mm.

[0075] The upper flange 21 is connected to the cover body 1. The cover body 1 is provided with a molten metal surface level sensor 7, an inert gas introduction valve 8 and a pressure reducing pump connection part 9.

[0076] Material: Aluminum-plated steel.

[0077] Casting operation 1: Before immersing the casting structure into the molten metal, an inert gas is introduced so that the inert gas fills the interior of the casting structure.

[0078] Casting operation 2: The lower half of the casting structure, about 500 mm, is placed in an electric furnace maintained at 700°C for 30 minutes of preheating. Afterwards, it is taken out of the electric furnace and slowly sunk into the molten metal while a certain amount of inert gas is continuously introduced. In addition, the molten metal temperature is 680°C.

[0079] Casting operation 3: After the casting mechanism is sunk to a position that is 10% of the height of the molten metal as calculated from the bottom, the pressure reducing pump is operated to suck the molten metal into the mold tube body 2.

[0080] Casting operation 4: After confirming that the molten metal has risen from a part of the filter 6 to a height of 1,100 mm using the molten metal surface level sensor 7, the decompression pump is turned off.

[0081] Casting operation 5: The casting structure is fished out from the molten metal, and then the mold tube body 2 is subjected to indirect water cooling treatment to solidify the molten metal in the mold tube body 2.

[0082] Obtaining the casting material: After confirming that the entire casting mechanism has been sufficiently cooled, the casting material is squeezed out of the mold tube body 2 to the outside using a clamp, thereby preparing the casting material.

[0083] Inclusion evaluation: Evaluation was performed by ultrasonic testing. The evaluation results are shown in Table 1.

[0084] Evaluation of component segregation: The Zn content was measured at the upper and lower ends of the casting material using an ICP emission spectrometer. The measurement results are shown in Table 2.

[0085] Comparative Example 1

[0086] Use as Figure 2 Casting mechanism of the construction shown.

[0087] As for the type of magnesium alloy, Mg-2wt%Zn alloy was prepared and produced.

[0088] The structure of the casting mechanism is as follows: 1 is a stainless steel mold tube body 2 with an inner diameter of 30 mm and a length of 500 mm. The upper half of the mold tube body 2 is provided with a filter 6. The mold tube body 2 is placed in an electric furnace as a whole for preheating.

[0089] Casting operation 1: Preparation of molten metal The smelting furnace used is the smelting furnace that was immersed in the casting mechanism and prepared to obtain molten metal in Example 1. The molten metal was poured into the casting mechanism. The temperature of the molten metal was 680°C.

[0090] Casting operation 2: In order to remove the precipitated inclusions and mixed gas generated by the injection of molten metal from the molten metal, a 10-minute precipitation and static treatment is performed. The molten metal temperature is maintained at 670±10℃.

[0091] Casting operation 3: After the precipitation and standing are completed, the entire casting mold tube body 2 is taken out from the electric furnace and directly water-cooled to solidify the molten metal inside.

[0092] Obtaining the casting material: After confirming that the entire casting mechanism has been sufficiently cooled, remove the filter 6, slowly return the mold tube 2 to its original position and take out the casting material.

[0093] Inclusion evaluation: Evaluation was performed by ultrasonic testing. The evaluation results are shown in Table 1.

[0094] Evaluation of component segregation: The Zn content was measured at the upper and lower ends of the casting material using an ICP emission spectrometer. The measurement results are shown in Table 2.

[0095] Comparative Example 2

[0096] Use as Figure 2 Casting mechanism of the construction shown.

[0097] Regarding the type of magnesium alloy, Mg-2wt%Zn alloy was produced.

[0098] The structure of the casting mechanism is as follows: 1 is a stainless steel mold tube body 2 with an inner diameter of 30 mm and a length of 1000 mm. The upper half of the mold tube body 2 is provided with a filter 6. The mold tube body 2 is placed in an electric furnace as a whole for preheating.

[0099] Casting operation 1: Preparation of molten metal The smelting furnace used was the smelting furnace used to produce the molten metal of Example 1. The molten metal was poured into the present casting mechanism. The temperature of the molten metal was 680°C.

[0100] Casting operation 2: In order to remove the precipitated inclusions and mixed gas from the molten metal due to the injection of the molten metal, a 10-minute precipitation and static treatment is performed. The molten metal temperature is maintained at 670±10°C.

[0101] Casting operation 3: After the precipitation and standing are completed, the entire casting mold tube body 2 is taken out from the electric furnace and directly water-cooled to solidify the molten metal inside.

[0102] Obtaining casting material: After confirming that the entire casting mechanism has been sufficiently cooled, the filter 6 is removed and the mold tube 2 is slowly returned to its original position, but the casting material inside cannot be pulled out and the casting material cannot be prepared.

[0103] Comparative Example 3

[0104] Use as Figure 3 Casting mechanism of the construction shown.

[0105] Regarding the type of magnesium alloy, Mg-2wt%Zn alloy was produced.

[0106] The structure of the casting mechanism is as follows: 1 is a stainless steel mold tube body 2 with an inner diameter of 30 mm and a length of 1000 mm. The mold tube body 2 is a cut-type structure that can be divided into two parts. The upper half of the mold tube body 2 has a filter 6. The mold tube body 2 is placed in an electric furnace as a whole for preheating.

[0107] Casting operation 1: Preparation of molten metal The smelting furnace used was the smelting furnace used to produce the molten metal of Example 1. The molten metal was poured into the present casting mechanism. The temperature of the molten metal was 680°C.

[0108] Casting operation 2: In order to remove the precipitated inclusions and mixed gases generated by the injection of molten metal from the molten metal, a 30-minute precipitation and static treatment is performed. The molten metal temperature is maintained at 670±10°C.

[0109] Casting operation 3: After the precipitation and standing are completed, the entire casting mold tube body 2 is taken out from the electric furnace and directly water-cooled to solidify the molten metal inside.

[0110] Obtaining the casting material: After confirming that the entire casting mechanism has been sufficiently cooled, remove the filter 6, disassemble the mold tube 2, and then take out the casting material.

[0111] Inclusion evaluation: Evaluation was performed by ultrasonic testing. The evaluation results are shown in Table 1.

[0112] Evaluation of component segregation: The Zn content was measured at the upper and lower ends of the casting material using an ICP emission spectrometer. The measurement results are shown in Table 2.

[0113] Table 1

[0114] Number of detected peaks Example 1 ND Comparative Example 1 19 Comparative Example 2 Failed to successfully prepare casting material. Comparative Example 3 7

[0115] Table 2

[0116]

[0117] In summary, by utilizing the setting of the filter 6 in the casting mechanism of the present invention, the occurrence of inclusions, gas mixing and component segregation can be avoided, thereby producing a casting material of a medical magnesium alloy, preferably a casting material with a small diameter and a longer size. In addition, the casting mechanism of the present invention can be subsequently installed on the existing smelting casting mechanism. In addition, since the molten metal is covered by the steel pipe, the molten metal liquid will not leak under inappropriate casting conditions like the semi-continuous casting casting mechanism, thereby causing water vaporization explosion, fire and other dangers. Compared with the traditional magnesium alloy casting casting mechanism, the operation of the casting mechanism does not require a wide space.

[0118] In summary, the present invention effectively overcomes various shortcomings of the prior art and has high industrial utilization value.

[0119] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A casting mechanism for medical magnesium alloy, It is characterized in that The invention comprises a cover body (1), a casting mold tube body (2), a filter clamp seat (3), a connecting tube body (4) and a bottom plate (5) which are connected in sequence from top to bottom, wherein a filter (6) is arranged in the filter clamp seat (3), and a molten metal surface level sensor (7), an inert gas introduction valve (8) and a pressure reducing pump connecting part (9) are respectively arranged on the cover body (1).

2. The casting mechanism of the medical magnesium alloy according to claim 1, It is characterized in that The inner diameter of the casting mold tube body (2) is 30±5 mm; the wall thickness of the casting mold tube body (2) is 2±1 mm; and the length of the casting mold tube body (2) is 500 to 1500 mm.

3. The casting mechanism of the medical magnesium alloy according to claim 1, It is characterized in that The casting mold tube body (2) is provided with an upper flange (21), and the cover body (1) and the casting mold tube body (2) are connected via the upper flange (21).

4. The casting mechanism of the medical magnesium alloy according to claim 1, It is characterized in that The casting mold tube body (2) is provided with a lower flange (22), and the filter clamp seat (3) and the casting mold tube body (2) are connected via the lower flange (22).

5. The casting mechanism of the medical magnesium alloy according to claim 1, It is characterized in that The filter holder (3) comprises an opening portion (31), and the filter (6) is arranged in the opening portion (31); the surface area of ​​the bottom plate (5) is greater than the surface area of ​​the opening portion (31).

6. The casting mechanism of the medical magnesium alloy according to claim 1, It is characterized in that The filter (6) is made of a material that does not react with the magnesium alloy molten metal.

7. The casting mechanism of the medical magnesium alloy according to claim 1, It is characterized in that The pore size of the filter (6) gradually decreases from an end close to the connecting tube body (4) to an end close to the casting mold tube body (2).

8. The casting mechanism of the medical magnesium alloy according to claim 1, It is characterized in that The distance between the filter clamping seat (3) and the bottom plate (5) is 15±10 mm.

9. The casting mechanism of the medical magnesium alloy according to claim 1, It is characterized in that The molten metal surface level sensor (7), the inert gas introduction valve (8) and the pressure reducing pump connection part (9) are respectively connected to the casting mold pipe body (2).

10. A method for preparing a casting material using a casting mechanism of a medical magnesium alloy as claimed in any one of claims 1 to 9, It is characterized in that The steps include: 1) introducing an inert gas into the casting mold tube body (2) through an inert gas introduction valve (8); 2) preheating the casting mold tube (2) and sinking the casting mechanism into the molten metal; 3) turning on the pressure reducing pump connected to the pressure reducing pump connection part (9) to suck the molten metal into the casting mold tube body (2); 4) after confirming that the molten metal has risen to a certain height from a portion of the filter (6) using the molten metal surface level sensor (7), the pressure reducing pump is turned off; 5) The casting mechanism is removed from the molten metal, and the mold tube body (2) is cooled so that the mold tube body (2) The molten metal inside solidifies; 6) The solidified molten metal is taken out to obtain a casting material.