Grinding magnetic needle and preparation method and application thereof

By using a grinding magnetic needle with a uniformly distributed adhesive layer and ceramic layer on the outer side of the magnetic needle body, the problems of poor polishing effect and corrosion in magnetic polishing technology are solved, achieving efficient surface polishing and corrosion-free treatment of hard metals.

CN118990138AActive Publication Date: 2024-11-22SICHUAN WEIJIA ADDITIVE MFG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411264272.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-22
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

The polishing medium material used in existing magnetic polishing technology is stainless steel, which has poor polishing effect and may cause corrosion of parts during service.

Method used

A method for preparing a grinding magnetic needle is adopted, in which an adhesive layer and a ceramic layer are evenly distributed on the outside of the magnetic needle body to form a grinding magnetic needle with magnetic conductivity and structural strength, which is used for surface polishing of hard metals in a magnetic polishing system.

Benefits of technology

It achieves efficient surface polishing of difficult-to-machine materials such as titanium alloys, high-temperature alloys, cobalt-chromium alloys, mold steel, and high-strength steel, avoiding polishing dead corners and corrosion during service.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005036696080000071
    Figure BDA0005036696080000071
  • Figure HDA0005036696090000011
    Figure HDA0005036696090000011
  • Figure HDA0005036696090000012
    Figure HDA0005036696090000012
Patent Text Reader

Abstract

The invention discloses a preparation method of a grinding magnetic needle. The preparation method comprises the following steps: selecting a needle-shaped magnetic needle body with magnetic conductivity; the magnetic needle bodies are evenly scattered into a container of a magnetic grinding machine, the magnetic field direction and the magnetic field intensity in the container are adjusted to enable the magnetic needle bodies to be kept vertical, and every two adjacent magnetic needle bodies are within a preset distance range; then at least one time of spraying work is conducted on the surface of the magnetic needle body, and each time of spraying work comprises the steps that firstly, high-temperature epoxy resin heated to 300-350 DEG C is evenly sprayed on the surface of the magnetic needle body to form a bonding layer; heating the interior of the container to at least 200 DEG C, and uniformly spraying ceramic particles on the bonding layer to form a ceramic layer; compared with the prior art, the grinding magnetic needle has the following advantages that the prepared grinding magnetic needle is applied to a magnetic polishing system to efficiently conduct surface polishing treatment on additive manufacturing structural parts formed by hard metal difficult to machine and efficiently conduct surface polishing treatment on various special-shaped curved surfaces and fine grooves without dead corners.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of precision machining of parts, and in particular to a grinding magnetic needle and a preparation method and application thereof. Background Art

[0002] Additive manufacturing is a technology that discretizes complex three-dimensional structural part models into two-dimensional structures and stacks them layer by layer. Therefore, its application in industrial fields such as aerospace, automobiles, and molds is increasing, facilitating rapid manufacturing to achieve lightweight, miniaturization, and integration of high-end equipment manufacturing. However, due to the temperature gradient and layer-by-layer forming process of additive manufacturing technology, the outer surface of the parts has half-burned or bonded powder particles, residual supports, and surface "step" effects.

[0003] At present, additively manufactured structural parts generally use surface polishing technology to eliminate sticky powder, residual support and polish the rough surface to meet the product assembly, service life and safety requirements. Some existing processes for surface treatment of additively manufactured structural parts have some problems, such as low efficiency of polishing the outer surface of additively manufactured structural parts by chemical reagent treatment; it is difficult to place contour electrodes in the dead corners of micro-pores and special-shaped surfaces of additively manufactured structural parts by electrochemical treatment, and polishing is impossible; contact polishing is limited by the freedom of the tool; abrasive flow polishing technology for internal flow channels is not suitable for polishing the outer surface of additively manufactured structural parts; water jets rely on the polishing medium ejected from micro nozzles to erode the material surface in a very small amount and range, and are usually used for polishing hard and brittle materials such as glass. The polishing efficiency of large-sized structural parts and additively manufactured surfaces that are too rough is low; magnetorheological polishing is limited by the magnetic field distribution and is only applicable to common polishing methods such as tubular and outer surface structures with regular directions. In addition, chemical methods such as chemical, electrochemical, and plasma polishing not only have a small removal amount and are difficult to improve the rough surface of additively manufactured structural parts on a large scale, but also produce a variety of corrosion and elemental pollution defects on additively manufactured structural parts. The corrosive liquid and reaction gas will also have adverse effects on the environment, people and equipment, and have been classified as restricted processes in the engine field.

[0004] In order to solve the above problems, magnetic polishing technology is generally used to perform surface polishing on additively manufactured structural parts. However, the materials of some additively manufactured structural parts are mainly difficult-to-process hard metals such as titanium alloys, high-temperature alloys, cobalt-chromium alloys, mold steels, and high-strength steels. The material of the polishing medium used in the magnetic polishing technology is generally stainless steel, and its polishing effect is very poor. In addition, for harder materials (such as high-temperature alloys), polishing may induce corrosion during the service process of the parts. Summary of the invention

[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a grinding magnetic needle and a preparation method and application thereof, so as to solve the problem in the prior art that the material of the polishing medium used in the magnetic polishing technology is generally stainless steel, the polishing effect is very poor and the polished material will also induce corrosion of the parts during service.

[0006] To achieve the above object, the first aspect of the present invention adopts the following technical solution: a method for preparing a ground magnetic needle, comprising the following steps:

[0007] Select a needle-shaped magnetic needle body with magnetic conductivity;

[0008] Evenly spread the magnetic needle bodies into the container of the magnetic grinding machine, and adjust the magnetic field direction and magnetic field strength in the container to keep the magnetic needle bodies vertical and keep two adjacent magnetic needle bodies within a preset distance range;

[0009] Then, at least one spraying operation is performed on the surface of the magnetic needle body, and each spraying operation includes:

[0010] To form an adhesive layer, firstly, a high-temperature epoxy resin heated to 300-350°C is evenly sprayed on the surface of the magnetic needle body to form an adhesive layer;

[0011] After forming the ceramic layer, the container is heated to at least 200° C., and then the ceramic particles are evenly sprayed on the bonding layer to form the ceramic layer.

[0012] The second aspect of the present invention adopts the following technical solution: a ground magnetic needle is prepared by the method for preparing a ground magnetic needle described in the first aspect of the present invention.

[0013] The third aspect of the present invention adopts the following technical solution: an application of a grinding magnetic needle, such as the application of a grinding magnetic needle as described in the second aspect of the present invention in a magnetic polishing system to polish a hard additively manufactured structural part.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] The preparation method of the grinding magnetic needle can stably and evenly distribute the adhesive layer and the ceramic layer on the outer side of the magnetic needle body in sequence, and the grinding magnetic needle formed by the combination has a needle-shaped and magnetically conductive magnetic needle body as the basic skeleton, and cooperates with the ceramic layer, so that the prepared grinding magnetic needle can have sufficient structural strength to be used in the magnetic polishing system to efficiently perform surface polishing treatment on additively manufactured structural parts formed of difficult-to-process hard metals such as titanium alloys, high-temperature alloys, cobalt-chromium alloys, mold steels, and high-strength steels, and can also efficiently perform surface polishing treatment on various special-shaped curved surfaces and fine grooves on additively manufactured structural parts to ensure that there are no polishing dead corners;

[0016] The outermost layer of the grinding magnetic needle prepared by the preparation method of the grinding magnetic needle is a ceramic layer. When the surface of the additively manufactured structural part is polished, no corrosion will occur during the service process of the additively manufactured structural part. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the movement of the nozzle during the spraying process of the present invention;

[0018] Figure 2 This is a layout diagram of the magnetic needle body in the container of the present invention;

[0019] Figure 3 An optical photograph of a cross-sectional view of a ground magnetic needle prepared in the present invention;

[0020] Figure 4 An optical photograph of the side surface of the ground magnetic needle prepared by the present invention;

[0021] Figure 5 A schematic diagram of a grinding magnetic needle size detection scheme prepared by the present invention;

[0022] Figure 6 This is a comparison chart of the effects of grinding and polishing a titanium alloy additive manufacturing method using a grinding magnetic needle prepared by the present invention and a traditional magnetic needle. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below through specific embodiments:

[0024] like Figure 1 As shown, a method for preparing a ground magnetic needle according to an embodiment of the present invention comprises the following steps:

[0025] Step s1, selecting a needle-shaped magnetic needle body with magnetic conductivity;

[0026] Step s2, evenly scattering the magnetic needle bodies into the container of the magnetic grinding machine, adjusting the direction and strength of the magnetic field in the container so that the magnetic needle bodies are kept vertical and two adjacent magnetic needle bodies are within a preset spacing range;

[0027] Step s3, then spraying the surface of the magnetic needle body at least once, each spraying operation includes:

[0028] Step s31, forming an adhesive layer, firstly spraying a high-temperature epoxy resin heated to 300-350° C. evenly on the surface of the magnetic needle body to form an adhesive layer;

[0029] Step s32, forming a ceramic layer, then heating the container to at least 200°C, and then spraying ceramic particles evenly on the adhesive layer to form a ceramic layer.

[0030] The preparation method of the ground magnetic needle can stably and evenly distribute the adhesive layer and the ceramic layer on the outer side of the magnetic needle body in sequence, and the ground magnetic needle (such as Figure 3 and Figure 4 ) A needle-shaped magnetic needle body with magnetic conductivity is used as the basic skeleton, and a ceramic layer is used to make the prepared grinding magnetic needle have sufficient structural strength to be used in a magnetic polishing system to move under the action of a magnetic field, so as to realize efficient surface polishing of additively manufactured structural parts formed of difficult-to-process hard metals such as titanium alloy, high-temperature alloy, cobalt-chromium alloy, mold steel, and high-strength steel in the magnetic polishing system, and can also efficiently perform surface polishing on various special-shaped curved surfaces and fine grooves on the additively manufactured structural parts to ensure that there are no polishing dead corners; the outermost layer of the grinding magnetic needle prepared by the preparation method of the grinding magnetic needle is a ceramic layer, and during the surface polishing of the additively manufactured structural parts, no corrosion will be generated during the service process of the additively manufactured structural parts.

[0031] In this embodiment:

[0032] In step s1:

[0033] The magnetic needle body is made of wire through tool punching or wire cutting. The wire material can be selected from stainless steel materials such as 304, 316 or 230, so that the magnetic needle body has good magnetic conductivity; here, the material of the magnetic needle body is not limited to any magnetic material.

[0034] Specifically, a magnetic needle body with a diameter of d=0.1mm~5mm and a length of 1mm~10mm is selected, which can achieve effective contact and processing of the outer surface of irregular and complex structures and micro-pores and grooves. At the same time, it can move under the action of the magnetic field in the magnetic polishing system to improve the polishing effect.

[0035] In step s2:

[0036] After the magnetic needle bodies are evenly scattered into the container of the magnetic grinder, the magnitude and direction of the electromagnetic coil current in the container of the magnetic grinder are set to achieve the set magnetic field strength and magnetic field direction formed in the container of the magnetic grinder; wherein the electromagnetic coil current is generally set in the range of 1 to 10A to make the magnitude of the magnetic field strength in the range of 0.30 to 1.0T; and then the magnetic needle bodies are arranged in the vertical direction in the container of the magnetic grinder and the spacing between adjacent magnetic needle bodies is 1 to 5mm (such as Figure 2 ). This is conducive to the uniform distribution during the subsequent spraying of high-temperature epoxy resin and ceramic particles.

[0037] In step s31:

[0038] First, heat the high-temperature epoxy resin (epoxy value 0.25-0.45) to 300-350°C. Specifically, by observing the flow state of the high-temperature epoxy resin after heating, it has a certain fluidity and can be sprayed out by the spray equipment to adhere to the outer surface of the magnetic needle body. Among them, the heating temperature of the high-temperature epoxy resin is 300°C, 310°C, 320°C, 330°C, 340°C or 350°C, etc. During the heating process, the high-temperature epoxy resin is first heated to 300°C, and its state is observed to determine whether it is necessary to increase its heating temperature. In the actual experimental process, it is found that the heating temperature of the high-temperature epoxy resin will not exceed 350°C to meet the use requirements.

[0039] Then, a glue spray nozzle with a length of 20 cm and a width of 1 cm is installed on the spray equipment, and the spray angle of the glue spray nozzle is designed to be 45°~75°, which can be 45°, 50°, 55°, 60°, 65°, 70° or 75°, etc.; and the spray pressure of the spray equipment is set to 0.03~0.1MPa, which can be 0.03MPa, 0.05MPa, 0.08MPa or 0.1MPa, etc. The design of this spray angle is to ensure that the small spacing of 1~5mm between adjacent magnetic needle bodies can be evenly sprayed with high-temperature epoxy resin to completely cover; and to ensure that the distance between the glue spray nozzle of the spray equipment and the top of the magnetic needle body is 2cm to prevent the heated high-temperature epoxy resin from solidifying due to the long spray distance, resulting in the inability to spray. Then run the spraying equipment to make the glue spray nozzle move from point 0 to point P at a speed of 38-52 cm / min on the x-axis, then move in the opposite direction to point P' and then move in the opposite direction back to point 0 to complete a spraying (such as Figure 1 );

[0040] The P point and the P' point are symmetrically arranged on the x-axis with the 0 point as the center, and the distance between the P point and the P' point is 200 cm in this embodiment, and the moving speed of the glue spray nozzle can be 38 cm / min, 40 cm / min, 42 cm / min, 44 cm / min, 46 cm / min, 48 cm / min, 50 cm / min or 52 cm / min, etc. At this moving speed, it is convenient for the high-temperature epoxy resin to densely cover the magnetic needle, ensuring the uniformity of the formation of the bonding layer.

[0041] During the spraying process, the current of the electromagnetic coil can be periodically changed between 1 and 10A at a speed of 4A per minute to make the magnetic needle body shake continuously in the container. The above-mentioned spraying path and parameter setting are combined to ensure that the surface of the magnetic needle body can be evenly coated with high-temperature epoxy resin to form a uniformly distributed adhesive layer.

[0042] In step s32:

[0043] Heat the temperature in the container to 200°C, clean the spray equipment and then load the ceramic particles into it, replace the sandblasting nozzle with a length of 20 cm and a width of 1 cm for the spray equipment, and design the spray angle of the sandblasting nozzle to be 45°~75°, specifically 45°, 50°, 55°, 60°, 65°, 70° or 75°, etc.; and set the spray pressure of the spray equipment to 0.05~0.3MPa, specifically 0.05MPa, 0.08MPa, 0.12MPa, 0.15MPa, 0.2MPa, 0.25MPa or 0.3MPa, etc.; and ensure that the distance between the sandblasting nozzle of the spray equipment and the top of the magnetic needle body is 2cm.

[0044] Then run the spraying equipment to make the sandblasting nozzle move from point 0 to point P at a speed of 38-52 cm / min on the x-axis, then move in the opposite direction to point P' and then move in the opposite direction back to point 0 to complete a spraying (such as Figure 1 );

[0045] Among them, the point P and the point P' are arranged symmetrically with the point 0 as the center on the x-axis, and the distance between the point P and the point P' is 200 cm in this embodiment. The moving speed of the sandblasting nozzle can be 38 cm / min, 40 cm / min, 42 cm / min, 44 cm / min, 46 cm / min, 48 cm / min, 50 cm / min or 52 cm / min, etc.

[0046] During the spraying process, the current of the electromagnetic coil can be periodically changed between 1 and 10A at a speed of 4A per minute to make the magnetic needle body shake continuously in the container. The above-mentioned spraying path and parameter setting are then combined to ensure that the outer surface of the semi-solid adhesive layer can be evenly wrapped with ceramic particles to form a uniformly distributed ceramic layer.

[0047] In the above, the material of the ceramic layer is one or more combinations of chrome corundum, diamond, boron nitride, aluminum oxide, zirconium oxide, carbide and titanium nitride. It is ensured that the formed grinding magnetic needle has sufficient structural strength and can perform surface polishing on workpieces mainly made of difficult-to-process hard metals such as titanium alloy, high-temperature alloy, cobalt-chromium alloy, mold steel, high-strength steel, etc.

[0048] Preferably, the material of the ceramic layer is chrome corundum, the particle size of chrome corundum is 90-110 μm and its main component is Al 2 O 3 and Cr 2 O 3 , where Al 2 O 3 The mass proportion of Cr is 97.5%, 2 O 3The mass of chrome corundum accounts for 1.3%. Because the hardness of this chrome corundum is higher than that of most materials, it is highly applicable to polishing materials, and the quality of the polished materials is high after polishing. At the same time, it will not scratch the surface of metals with normal hardness such as titanium alloys and stainless steel due to excessive hardness.

[0049] It should be noted that: multiple spraying operations can be performed on the surface of the magnetic needle body according to demand, and multiple adhesive layers and multiple ceramic layers are alternately arranged on the outer surface of the magnetic needle body, and the outermost layer is always the ceramic layer. Among them, in order to further improve the more uniform distribution of adhesive layers and ceramic layers on the magnetic needle body, when the nozzle moves to point P and point P' on the x-axis, it is necessary to change the direction of the electromagnetic coil current in the container of the magnetic grinder, thereby changing the direction of the magnetic field, so that the original N pole becomes the S pole, and the original S pole becomes the N pole, so as to change the direction of the magnetic needle body in the container and reduce the spraying dead angle caused by the contact between the magnetic needle body and the inner wall of the container.

[0050] The ground magnetic needle prepared by this method has high grinding force and grinding efficiency. It is aimed at the precise requirements of size, roughness and removal amount of the outer surface of the complex and irregular structure after polishing in additive manufacturing. Based on the theory of external circle cutting-in grinding surface and the engineering data accumulated in actual processing, an empirical formula between the removal amount, roughness and processing time process parameters of different materials is established to meet the needs of process parameter control when precise requirements of size, roughness and removal amount are met under different materials.

[0051] For example, the size measurement of the crescent groove using a microscope is used to determine the amount of groove wall removed during magnetic grinding. Figure 5 As shown, Φ is measured respectively. max , l min , l′ min Three sizes. Φ max It is the maximum diameter in the middle of the crescent groove, measured by drawing a circle between two tangent points under a microscope. The length of the arc AB on the left is recorded as l min , the length of the arc A′B′ on the right is recorded as l′ min The arc length is measured by the microscope arc length tool. Specifically, a circle with a radius of 1 mm is made with the crescent tip as the center, intersecting the crescent groove at points AB and A′B′. Detect and record Φ max , l min , l′ min The values ​​of the three along with the processing time can obtain the bilateral removal data of the widest and narrowest parts of the crescent groove. The removal at the widest and narrowest parts of the crescent groove is selected as the characteristic data because these two places have the largest difference in magnetic needle abrasive flux and grinding effect.

[0052] Table 1 is the result of the size test of the composite magnetic needle after grinding. From the second hour onwards, the Φ max , l min , l′min Three sizes. It can be seen from the table that when the processing time reaches 6h, Φ max , l min , l′ min The three dimensions tend to be stable, among which the bilateral removal at the widest part of the middle of the crescent groove is 0.226mm, and the bilateral removal at the two corners of the crescent groove is 0.2mm and 0.207mm, indicating that the fixed abrasive can effectively grind and remove the high-temperature alloy material. The removal after 8 hours can reach the thickness of the remelted layer after EDM of 0.05mm to 0.2mm. However, there is still a decrease in grinding efficiency after 6 hours and the removal tends to the limit. At the same time, the bilateral removal at the widest part of the middle of the crescent groove and the two corners of the crescent groove differ by about 2 times. This is because the larger the abrasive flux, the better the grinding effect.

[0053] Table 1 Dimensional test results of composite magnetic needle after grinding

[0054]

[0055] The grinding magnetic needle prepared by this method and the traditional magnetic needle (i.e., the magnetic needle body in this method) are respectively applied to the magnetic polishing system to grind and polish the outer surface of a titanium alloy additive manufacturing. The effect after grinding and polishing is shown in the figure Figure 6 , Figure 6 The left side of the figure shows the effect of using a traditional magnetic needle in a magnetic polishing system to grind and polish the outer surface of titanium alloy additive manufacturing. Figure 6 The right side of the figure shows the effect of using a traditional magnetic needle in a magnetic polishing system to grind and polish the outer surface of titanium alloy additive manufacturing.

[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a ground magnetic needle, It is characterized in that The following steps are involved: Select a needle-shaped magnetic needle body with magnetic conductivity; Evenly spread the magnetic needle bodies into the container of the magnetic grinding machine, and adjust the magnetic field direction and magnetic field strength in the container to keep the magnetic needle bodies vertical and keep two adjacent magnetic needle bodies within a preset distance range; Then, at least one spraying operation is performed on the surface of the magnetic needle body, and each spraying operation includes: To form an adhesive layer, firstly, a high-temperature epoxy resin heated to 300-350°C is evenly sprayed on the surface of the magnetic needle body to form an adhesive layer; After forming the ceramic layer, the container is heated to at least 200° C., and then the ceramic particles are evenly sprayed on the bonding layer to form the ceramic layer.

2. A method for preparing a ground magnetic needle according to claim 1, Features: In the process of forming the bonding layer or the ceramic layer, a spraying device is used for spraying, and the nozzle of the spraying device is sprayed in the following motion mode during spraying: The nozzle of the spraying device moves from point 0 to point P at a moving speed of 38 to 52 cm / min on the x-axis, then moves in the reverse direction to point P′, and then moves in the reverse direction back to point 0 to complete a spraying operation; The point P and the point P′ are symmetrically arranged on the x-axis with the point 0 as the center.

3. A method for preparing a ground magnetic needle according to claim 2, Features: During the process of forming the adhesive layer, the spray pressure of the spray equipment is 0.03-0.1 MPa, the distance between the nozzle of the spray equipment and the top of the magnetic needle body is 2 cm, and the spray angle of the nozzle of the spray equipment is 45°-75°.

4. A method for preparing a ground magnetic needle according to claim 2, Features: During the process of forming the ceramic layer, the spray pressure of the spray equipment is 0.05-0.3 MPa, the distance between the nozzle of the spray equipment and the top of the magnetic needle body is 2 cm, and the spray angle of the nozzle of the spray equipment is 45°-75°. 5 . The method for preparing a ground magnetic needle according to claim 1 , wherein the diameter of the magnetic needle body is d=0.1 mm to 5 mm and the length thereof is 1 mm to 10 mm.

6. According to the method for preparing a ground magnetic needle according to claim 1, the magnetic needle body is made of wire material by tool punching or wire cutting.

7. The method for preparing a ground magnetic needle according to claim 1, wherein the material of the ceramic layer is one or more combinations of chrome corundum, diamond, boron nitride, aluminum oxide, zirconium oxide, carbide and titanium nitride.

8. The method for preparing a ground magnetic needle according to claim 7, wherein the material of the ceramic layer is chrome corundum, the particle size of chrome corundum is 90-110 μm and its main component is Al 2 O 3 and Cr 2 O 3 .

9. A grinding magnetic needle, It is characterized in that The invention is prepared by the method for preparing a ground magnetic needle according to any one of claims 1 to 8.

10. An application of grinding magnetic needles, It is characterized in that The use of a grinding magnetic needle as described in claim 9 for polishing hard additively manufactured structural parts in a magnetic polishing system.