Continuous flat pressing manufacturing method for fast-curing polyurethane-based core-board
Through the continuous flat pressure manufacturing method of using solvent-free foamed polyurethane resin and high moisture content wood veneer in the production of joinery boards, the problems of high formaldehyde emission, low efficiency and single specifications in the production of joinery boards are solved, and the problem of high formaldehyde emission, low efficiency and single specifications are achieved. More efficient and environmentally friendly production process and excellent physical and mechanical properties.
Patent Information
- Application Number
- CN202411272738.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-11
AI Technical Summary
There are problems in the production of joinery boards with high formaldehyde emission, low production efficiency and single specifications.
Solvent-free foamed polyurethane resin is used as adhesive, and continuous core plate is formed through finger joint and horizontal splicing methods. Combined with veneer splicing technology, a continuous flat pressure manufacturing method is realized, and wood veneer and core with high moisture content is used. The board is sprayed with single-sided or double-sided adhesive, and is heat-pressed to improve production efficiency and product specifications.
It reduces production costs and energy consumption, expands the specifications of joinery boards, improves physical and mechanical properties, reduces formaldehyde emission and glue consumption, and improves production efficiency and product application range.
Smart Images

Figure CN118990709A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for continuously flat-pressing a fast-curing polyurethane-based blockboard and belongs to the technical field of wood processing. Background Art
[0002] Blockboard refers to a special type of plywood made by gluing and pressing wood strips or hollow boards as the core, and covering two or more layers of plywood on both sides. The characteristics of blockboard are mainly determined by the core structure. Blockboard has good screw holding power, high strength, and is strong, sound-absorbing, and heat-insulating. It is easy to process and is widely used in furniture manufacturing, interior decoration, carriages, ships, and other production and construction fields.
[0003] At present, the main problems existing in the production process of blockboard include: first, a large amount of formaldehyde series resin adhesives such as urea-formaldehyde resin are used in the production process of blockboard, which leads to the defect of high formaldehyde release during the production and use of blockboard; second, intermittent or periodic production methods are used, and the production efficiency is low; third, the format of blockboard products is relatively single. my country mainly produces two specifications of 1220mm×2440mm and 915mm×1830mm, which limits its application scope. Summary of the invention
[0004] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a method for continuously pressing and manufacturing a fast-curing polyurethane-based blockboard. The method of the present invention ensures that the formaldehyde emission of the prepared blockboard reaches the ENF level through reasonable selection of the adhesive, and also helps to improve the performance of the prepared blockboard.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows: 1. Preparation of solvent-free foamable polyurethane resin (1) Under stirring, 10 to 50 parts by weight of sucrose polyether tetraol and 100 parts by weight of polypropylene glycol are uniformly mixed to prepare a mixed polyether polyol, wherein the hydroxyl value of the mixed polyether polyol is 300 to 400 mgKOH / g; (2) dehydrating 300 parts by weight of polypropylene glycol at 110-130° C. for 120 minutes, cooling to 95° C. under stirring, adding polymethylene polyphenyl polyisocyanate, reacting at 85-95° C. for 120 minutes, and cooling to obtain a prepolymer, wherein the isocyanate group content of the prepolymer is 1-3%; (3) 100 parts by weight of a mixed polyether polyol, 1.5 parts by weight of an organosilicon foam stabilizer, 0.1 parts of dibutyltin dilaurate, 10 to 50 parts by weight of a prepolymer, 100 parts by weight of polymethylene polyphenyl polyisocyanate, and 10 parts by weight of cyclohexanone are mixed and stirred to obtain a solvent-free foamable polyurethane resin; the curing speed of the polyurethane resin is 40 to 90 seconds; 2. Finger-joined and horizontally spliced slats are used to make core boards. When finger-joined slats are horizontally spliced, the finger joints are staggered and do not overlap. The core boards are finger-joined vertically spliced on the production line to form a continuous core board with a moisture content of 8-20%; 3. The wood veneer with a thickness of 1.5-5.0 mm is spliced by a veneer splicing method to obtain a continuous wood veneer with a moisture content of 8-20%; 4. Use solvent-free foaming polyurethane resin as adhesive, apply adhesive on continuous core board and continuous wood veneer, lay continuous wood veneer on both sides of continuous core board to make continuous blockboard blank, hot press and shear to obtain blockboard of required specifications, wherein the wood grain of core board is parallel to the direction of production line, and the wood grain of wood veneer is perpendicular to the direction of production line.
[0006] The adhesive coating method is single-sided spraying or double-sided roller coating. The wood veneer is coated with glue on one side, and the coated surface is the surface in contact with the core board; the core board is coated with glue on both sides of the roller, and the coated surface is the surface in contact with the wood veneer. The amount of glue is 250-300g / m 2 ; The hot pressing temperature is 50~190℃, the pressure is 1.0~1.5MPa, and the hot pressing factor is 10~50s / mm.
[0007] The advantages and technical effects of the present invention are as follows: 1. Reduce labor costs in the production process of blockboard and improve production efficiency. Traditional blockboard core board and wood veneer surface board assembly rely heavily on manual labor. The present invention realizes the automation and continuous assembly of blockboard core board and wood veneer surface board, which not only saves labor costs but also improves production efficiency; when using a medium-temperature curing production process, it can reduce energy consumption in the production process; the present invention uses solvent-free foaming polyurethane resin to replace traditional formaldehyde series resins. After the polyurethane is cured, the molecular structure is stable and there is no problem of formaldehyde release; 2. Expanded blockboard specifications. Since the products coming out of the hot press are continuous, they can be cut to any length, and the product specifications are more diverse, especially the length specifications; 3. The physical and mechanical properties of the blockboard are better. By adjusting the polyurethane resin formula and the thickness of the wood veneer, the static bending strength and nail holding force of the blockboard can be adjusted to ensure that the physical and mechanical properties of the blockboard of the present invention are better. Since the oriented strand board and the blockboard core board have the same wood grain arrangement characteristics, the technology of the present invention can be used for blockboard products with oriented strand board as the base material; 4. The present invention uses foaming adhesive technology to reduce glue consumption during the production process. In order to improve the production efficiency of blockboard, the curing speed of polyurethane is increased by using mixed polyether polyols and prepolymer preparation methods, and the proportion is adjusted to meet different hot pressing temperature requirements; blockboard and wood veneer with higher moisture content are used in the manufacturing process, which improves the drying production efficiency and reduces the damage during the drying process. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 It is a schematic diagram of a joinery core board with staggered joints of the slats of the present invention; Figure 2 It is a schematic diagram of the process of preparing the blockboard by single-sided glue spraying and continuous flat pressing of the present invention; Figure 3 It is a schematic diagram of the process of preparing the blockboard by double-sided roller gluing and continuous flat pressing of the present invention; Figure 4 It is a schematic diagram of the continuous flat pressing preparation process of the glue coating in Example 3. DETAILED DESCRIPTION
[0009] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0010] The rapid curing polyurethane-based blockboard continuous flat pressing manufacturing method of the present invention combines the performance advantages of polyurethane resin and the efficiency advantages of the continuous flat pressing production method. The manufacturing process also fully absorbs the advantages of various existing blockboard production technologies. Compared with the existing intermittent production method, it is more efficient.
[0011] The core board of the present invention is a relatively independent manufacturing unit, which is produced in a conventional production line according to conventional technology and is used for subsequent manufacturing.
[0012] Example 1: Method for manufacturing 915 mm wide rapid curing polyurethane-based blockboard by continuous flat pressing 1. Preparation of core board (1) Finger-joint the 15 mm thick, 610 mm long, and 20% moisture content laths to obtain 1830 mm long laths; (2) Length 1830mm Figure 1 Arrangement mode: horizontal splicing to obtain core board; 2. Preparation of wood veneer The wood segment with a length of 915 mm is peeled to obtain a transverse wood veneer with a thickness of 1.5 mm, a width of 915 mm and a moisture content of 20%; 3. Preparation of solvent-free foamable polyurethane resin (1) Under stirring, 50 parts of sucrose polyether tetraol and 100 parts of polypropylene glycol are uniformly mixed to prepare a mixed polyether polyol, wherein the hydroxyl value of the mixed polyether polyol is 400 mgKOH / g; (2) Add 300 parts of polypropylene glycol to a reaction kettle, dehydrate at 120°C for 120 minutes, cool to 95°C with stirring, add an appropriate amount of polymethylene polyphenyl polyisocyanate, and keep the reaction at 90°C for 120 minutes, then cool to obtain a prepolymer. The isocyanate group content in the prepolymer is 3%; (3) 100 parts of mixed polyether polyol, 1.5 parts of silicone foam stabilizer, 0.1 parts of dibutyltin dilaurate, 50 parts of prepolymer, 100 parts of polymethylene polyphenyl polyisocyanate, 10 parts of cyclohexanone, etc. were stirred and mixed uniformly to prepare a solvent-free foamable polyurethane resin; the curing speed of the polyurethane resin was 40 seconds; 4. Continuous splicing of joinery core layer and wood veneer Use conventional splicing technology to achieve continuous splicing of core board and wood veneer, where the core board is finger-joined longitudinally on the production line; 5. Gluing Solvent-free foaming polyurethane resin is used as adhesive. The upper and lower surfaces of the wood veneer are coated with glue on one side by using a single-sided spray (spray) method. The coated surface is the surface in contact with the core board of the joinery. The single-sided glue coating amount is 250~300g / m 2 ( Figure 2 ); 6. Histogenesis The glued lower surface veneer, the core board and the glued upper surface veneer are laid in sequence to obtain a continuous blockboard blank, wherein the wood texture of the core board is parallel to the traveling direction of the production line, and the wood texture of the wood veneers on the upper and lower surfaces is perpendicular to the traveling direction of the production line; the blockboard blank is continuously hot-pressed at a temperature of 50°C, a pressure of 1.0-1.5MPa, and a hot pressing factor of 10s / mm, and after being cut, a blockboard product with specified specifications is obtained.
[0013] The performance of the finished blockboard was tested, and the results are shown in Table 1.
[0014] Example 2: Method for manufacturing 1220 mm wide rapid curing polyurethane-based blockboard by continuous flat pressing 1. Preparation of core board (1) Finger-joint the joinery strips with a thickness of 8 mm, a length of 610 mm and a moisture content of 8% to obtain strips with a length of 2440 mm; (2) Length 2440mm Figure 1 Arrangement mode: horizontal splicing to obtain core board; 2. Preparation of wood veneer The wood segments with a length of 1220 mm were peeled to obtain cross-grained wood veneers with a thickness of 5 mm, a width of 1220 mm, and a moisture content of 8%; 3. Preparation of solvent-free foamable polyurethane resin (1) Under stirring, 10 parts of sucrose polyether tetraol and 100 parts of polypropylene glycol are uniformly mixed to prepare a mixed polyether polyol, wherein the hydroxyl value of the mixed polyether polyol is 300 mgKOH / g; (2) Add 300 parts of polypropylene glycol to a reaction kettle, dehydrate at 120°C for 120 minutes, cool to 95°C with stirring, add an appropriate amount of polymethylene polyphenyl polyisocyanate, and keep the reaction at 90°C for 120 minutes, then cool to obtain a prepolymer. The isocyanate group content in the prepolymer is 1%; (3) 100 parts of mixed polyether polyol, 1.5 parts of silicone foam stabilizer, 0.1 parts of dibutyltin dilaurate, 10 parts of prepolymer, 100 parts of polymethylene polyphenyl polyisocyanate, 10 parts of cyclohexanone, etc. were stirred and mixed to obtain a solvent-free foamable polyurethane resin; the curing speed of the polyurethane resin was 90 seconds; 4. Continuous splicing of core board and wood veneer Use conventional splicing technology to achieve continuous splicing of core board and wood veneer, where the core board is finger-joined longitudinally on the production line; 5. Gluing Solvent-free foaming polyurethane resin was used as adhesive. Double-sided roller gluing was used to apply glue to both sides of the core board. The glued surface was the surface in contact with the wood veneer. The amount of glue applied on one side was 250-300 g / m 2 ( Figure 3 ); 6. Histogenesis The lower surface veneer, the glue-coated core board and the upper surface veneer are laid in sequence to obtain a continuous core board blank, wherein the wood texture of the core board is parallel to the traveling direction of the production line, and the wood texture of the wood veneers on the upper and lower surfaces is perpendicular to the traveling direction of the production line; the core board blank is continuously hot-pressed at a temperature of 180°C, a pressure of 1.0-1.5MPa, and a hot pressing factor of 50s / mm, and after being cut, a core board product with specified specifications is obtained.
[0015] The performance of the finished blockboard was tested, and the results are shown in Table 1.
[0016] Example 3: Method for manufacturing continuous flat pressing of blockboard with a width of 1220 mm fast-curing polyurethane-based oriented strand board substrate 1. Preparation of oriented strand board According to the conventional oriented strand board production technology, a conventional oriented strand board with a thickness of 15 mm is obtained; 2. Preparation of wood veneer The wood segment with a length of 1220 mm is peeled to obtain a cross-grained wood veneer with a thickness of 1.5 mm, a width of 1220 mm and a moisture content of 8%; 3. Preparation of solvent-free foamable polyurethane resin (1) Under stirring, 25 parts of sucrose polyether tetraol and 100 parts of polypropylene glycol are uniformly mixed to prepare a mixed polyether polyol, wherein the hydroxyl value of the mixed polyether polyol is 300 mgKOH / g; (2) Add 300 parts of polypropylene glycol to a reaction kettle, dehydrate at 120°C for 120 minutes, cool to 95°C with stirring, add an appropriate amount of polymethylene polyphenyl polyisocyanate, and keep the reaction at 90°C for 120 minutes, then cool to obtain a prepolymer. The isocyanate group content in the prepolymer is 2%; (3) 100 parts of mixed polyether polyol, 1.5 parts of silicone foam stabilizer, 0.1 parts of dibutyltin dilaurate, 25 parts of prepolymer, 100 parts of polymethylene polyphenyl polyisocyanate, 10 parts of cyclohexanone, etc. were stirred and mixed uniformly to prepare a solvent-free foamable polyurethane resin; the curing speed of the polyurethane resin was 65 seconds; 4. Continuous splicing of oriented strand board core layer and wood veneer The core board is an oriented strand board produced by a continuous flat pressing process, wherein the adhesive used in the manufacturing process of the oriented strand board is a non-formaldehyde adhesive, and conventional splicing technology is used to achieve continuous splicing of wood veneers for the upper and lower surfaces; 5. Gluing Solvent-free foaming polyurethane resin is used as adhesive. Wood veneer and oriented strand board are coated with glue at the same time. The wood veneer is coated with glue on one side, and the coated side is the surface in contact with the oriented strand board. The core layer of the oriented strand board is sanded and then coated with glue by double-sided rollers. The coated side is the surface in contact with the wood veneer. The single-sided glue coating amount is 250~300g / m 2 ( Figure 4 ); 6. Histogenesis The lower surface wood veneer, the glue-coated oriented strand board and the upper surface wood veneer are laid in sequence to obtain a continuous blockboard blank, wherein the wood texture of the core board is parallel to the traveling direction of the production line, and the wood texture of the wood veneers on the upper and lower surfaces is perpendicular to the traveling direction of the production line; the blockboard blank is continuously hot-pressed at a temperature of 90°C, a pressure of 1.0-1.5MPa, and a hot pressing factor of 30s / mm, and after being cut, a blockboard product with an oriented strand board substrate of specified specifications is obtained.
[0017] The performance of the finished blockboard was tested, and the results are shown in Table 1.
[0018] Table 1
[0019] Note: In this implementation, the source of formaldehyde release is the extract from wood.
Claims
1. A method for manufacturing a fast-curing polyurethane-based blockboard by continuous flat pressing, characterized in that: Here are the steps: (1) The slats are made into core boards by finger-joining and horizontal splicing. When the finger-joined slats are horizontally spliced, the finger joints are staggered and do not overlap. The core boards are finger-joined vertically on the production line to form a continuous core board. (2) Using a veneer splicing method to obtain a continuous wood veneer with a thickness of 1.5 to 5.0 mm; (3) Using solvent-free foaming polyurethane resin as adhesive, after coating the adhesive on the continuous core board and the continuous wood veneer, the continuous wood veneer is laid on the upper and lower surfaces of the continuous core board to obtain a continuous blockboard blank, which is then hot-pressed and sawn to obtain blockboards of required specifications, wherein the wood grain of the core board is parallel to the direction of travel of the production line, and the wood grain of the wood veneer is perpendicular to the direction of travel of the production line.
2. The method for manufacturing fast-curing polyurethane-based blockboard by continuous flat pressing according to claim 1, characterized in that: The preparation method of solvent-free foamable polyurethane resin is as follows: (1) Under stirring, 10 to 50 parts by weight of sucrose polyether tetraol and 100 parts by weight of polypropylene glycol are uniformly mixed to prepare a mixed polyether polyol, wherein the hydroxyl value of the mixed polyether polyol is 300 to 400 mgKOH / g; (2) dehydrating 300 parts by weight of polypropylene glycol at 110-130° C. for 120 minutes, cooling to 95° C. under stirring, adding polymethylene polyphenyl polyisocyanate, reacting at 85-95° C. for 120 minutes, and cooling to obtain a prepolymer, wherein the isocyanate group content of the prepolymer is 1-3%; (3) 100 parts by weight of a mixed polyether polyol, 1.5 parts by weight of an organosilicon foam stabilizer, 0.1 parts of dibutyltin dilaurate, 10 to 50 parts by weight of a prepolymer, 100 parts by weight of polymethylene polyphenyl polyisocyanate, and 10 parts by weight of cyclohexanone are mixed and stirred to obtain a solvent-free foamable polyurethane resin.
3. The method for manufacturing fast curing polyurethane-based blockboard by continuous flat pressing according to claim 1, characterized in that: The hot pressing temperature is 50~190℃, the pressure is 1.0~1.5MPa, and the hot pressing factor is 10~50s / mm.
4. The method for manufacturing fast curing polyurethane-based blockboard by continuous flat pressing according to claim 1, characterized in that: The moisture content of continuous core board and continuous wood veneer is 8~20%.
5. The method for manufacturing fast curing polyurethane-based blockboard by continuous flat pressing according to claim 1, characterized in that: The adhesive coating method is single-sided spray coating or double-sided roller coating, and the coating amount is 250~300g / m 2 .
6. The method for manufacturing fast curing polyurethane-based blockboard by continuous flat pressing according to claim 1, characterized in that: Oriented strand board is used as the core board.
7. The method for manufacturing fast curing polyurethane-based blockboard by continuous flat pressing according to claim 5, characterized in that: The wood veneer is coated with glue on one side by spraying, and the glue-coated surface is the surface in contact with the core board; the core board is coated with glue on both sides by roller, and the glue-coated surface is the surface in contact with the wood veneer.
Citation Information
Patent Citations
Fire resistant water resistant polyurethane composition for fluid sealant and manufacture method thereof
CN101245182A
Environment-friendly high-strength polyurethane adhesive sealant and preparation method thereof
CN103897652A
Zero-formaldehyde-release waterborne Muxiang board and preparing method thereof
CN106827106A
Zero-formaldehyde release water-borne polyurethane adhesive LVL (Laminated Veneer Lumber) and manufacturing method thereof
CN107309983A
Pre-pressing type veneer ultrathin large shaving board composite core-board and manufacturing method thereof
CN114919031A
Cited By
Mixed artificial board and preparation method and application thereof
CN119682003A