Super-strong bamboo wood and preparation method thereof
By performing two-step treatment on natural bamboo, lignin is removed and cellulose macromolecules are promoted to form a dense structure, which solves the problem of low tensile strength of bamboo, and achieves high-strength and environmentally friendly bamboo preparation, which is suitable for modern application needs.
Patent Information
- Application Number
- CN202411262750.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art lacks simple, effective, environmentally friendly and excellent mechanical properties to prepare lightweight, high-strength super-strong bamboo, and the tensile strength of the bamboo is low, making it difficult to meet the needs of modern applications.
By performing a two-step treatment of natural bamboo: first, use a strong alkali or other specific solution to remove lignin and expose the active hydroxyl groups on the surface of the fiber; second, dissolve part of the fiber in a suitable solution to promote the regeneration of cellulose macromolecules and the tightness between the fibers. Combined, a dense structure is formed, thereby improving the tensile strength of bamboo.
The tight bonding of bamboo fibers has been achieved, which significantly improves the tensile strength and the stress transmission effect between fibers, avoids stress concentration, and reaches a tensile strength of 1600MPa. The method is environmentally friendly and biodegradable, and is suitable for different sizes. Bamboo preparation.
Smart Images

Figure CN118990719A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a bamboo material and a preparation method thereof, in particular to a super-strong bamboo material and a preparation method thereof. Background Art
[0002] Lightweight structural materials with high strength play a huge role in advanced applications in transportation, construction, automobiles and aerospace. To meet modern needs, a large number of petroleum products (such as carbon fiber, carbon nanotubes and graphene), ceramics and metals have been fully developed and utilized. However, these materials often require complex and costly manufacturing processes and are prone to adverse effects on the environment. Therefore, people have paid more and more attention to low-cost bio-based materials with high environmental protection in order to solve the above problems. Among many natural materials, bamboo has attracted attention due to its significant structural and environmental advantages, including rapid growth, moisture resistance, climate tolerance and structural rigidity. However, due to the large number of defects inside bamboo, the natural brittleness of the lignin network and the weak interfacial interaction between thin-walled cells, the tensile strength of bamboo is only 300-400MPa, which is much lower than the theoretical mechanical strength of primary cellulose fibers (≈7.5GPa). Therefore, designing and manufacturing lightweight and high-strength bamboo materials remains a challenge.
[0003] Extensive research has been conducted to improve the mechanical properties of bamboo. Chinese patent CN112026213A discloses a method for manufacturing a super-strong bamboo fiber composite board. The method for manufacturing the composite board includes: mixing bamboo fiber and thermoplastic short fibers into a bamboo-plastic blended rope, then cross-arranging them at a certain angle according to the "warp" and "weft", and finally fully filling the mixed powder composed of thermoplastic powder and bamboo fiber powder, and hot pressing it. The bonding effect of thermoplastic materials under high temperature and high pressure is utilized to enhance the interaction between bamboo fiber and thermoplastic materials, enhance stress transfer when subjected to force, avoid stress concentration, and thus improve the mechanical properties of the board. This method mainly relies on improving the strength of bamboo through the bonding of thermoplastic materials. The winding of fibers and the filling of mixed powder are both for better bonding. Existing polymer adhesives can only bond the interface between the two through their own action. The preparation process is complicated and there is a hidden danger of environmental pollution.
[0004] Current technology lacks a simple, effective, environmentally friendly, and excellent mechanical property reinforcement method for bamboo. Therefore, it is urgent to successfully prepare an environmentally friendly, lightweight, high-strength, and expandable super-strong bamboo material. Summary of the invention
[0005] Purpose of the invention: The present invention aims to provide a super-strong bamboo material with high mechanical strength; the present invention also aims to provide a method for preparing the super-strong bamboo material.
[0006] Technical solution: The super-strong bamboo material described in the present invention includes micron-level delignified bamboo fibers and in-situ regenerated bamboo fibers. The bamboo fibers have a compact structure after delignification, the pores of the bamboo fibers are densely filled with in-situ regenerated bamboo fibers, and the bamboo fibers are tightly combined with the in-situ regenerated bamboo fibers to form a dense microstructure.
[0007] Preferably, the thickness of the super-strong bamboo material is 50-300 μm and the density is 1.4-2.0 g·cm -3 .
[0008] Preferably, the longitudinal tensile strength of the fibers of the super-strong bamboo material can reach 1300-1700 MPa, and the transverse tensile strength can reach 400-800 MPa.
[0009] The method for preparing the super-strong bamboo material comprises the following steps:
[0010] The natural bamboo material is immersed in a treatment solution A, delignified and washed to obtain a first intermediate; the treatment solution A is one or more of a strong alkaline solution, an acetic acid solution, a hydrogen peroxide solution, a sodium hypochlorite solution, and a sodium sulfite solution;
[0011] The first intermediate is immersed in a treatment solution B to dissolve part of the fiber to obtain a second intermediate; the treatment solution B is at least one of an alkali / urea mixed solution, a lithium chloride / NN dimethylacetamide solution, an N-methylmorpholine-N-oxide solution, an ion solution, and a cuprammonia solution;
[0012] The second intermediate is left to stand, then washed and dried to obtain the super-strong bamboo material.
[0013] Among them, the delignification treatment leaves larger pores between fibers, exposing more hydroxyl groups of the fibers. Based on this step, the partial dissolution of the surface of the micron fiber exposes more active hydroxyl groups. The dissolved part forms cellulose macromolecules and is distributed on the fibers and between the fibers and fiber bundles. As the dissolution system is destroyed (cleaning process), these evenly distributed cellulose macromolecules re-crystallize and regenerate in situ. The regenerated nano-cellulose has extremely rich hydroxyl groups. The rich active hydroxyl groups form a large number of hydrogen bonds during the drying process. They are like a natural adhesive that tightly bonds the fibers and fiber bundles. Such a dense structure greatly improves the tensile strength of bamboo. The close bonding between the fibers enables the bamboo to transfer stress more effectively when it is subjected to tension, avoiding the phenomenon of stress concentration on a single interface, better dispersing the force, and achieving a significant improvement in tensile strength.
[0014] Preferably, the natural bamboo material is derived from yellow bamboo, nan bamboo, green bamboo or bitter bamboo.
[0015] Preferably, the treatment solution A is a mixed solution of sodium hydroxide and sodium sulfite, and the treatment solution B is a lithium chloride / NN dimethylacetamide solution. The sodium hydroxide / sodium sulfite system can provide a mild delignification method for wood, while removing a large amount of lignin, the fiber structure is as little damaged as possible, thereby obtaining a bamboo material with the original strength maintained and the lignin removed as much as possible; the NN dimethylacetamide solution / lithium chloride can fully dissolve the surface of the micron fiber without destroying the internal structure of the fiber, so that the bamboo fiber can be more tightly bonded while maintaining its own strength.
[0016] Preferably, the mass ratio of the absolute dry mass of the natural bamboo material to the treatment solution A is 1 to 5:10, and the delignification treatment method comprises: soaking in the treatment solution A at 50 to 100° C. for 1 to 12 hours, and washing with water after delignification.
[0017] Preferably, the mass ratio of the absolute dry mass of the delignified bamboo material to the B treatment solution is 1:5-50.
[0018] Preferably, the treatment temperature of the treatment solution B is -20 to 200°C, and the treatment time is 10 minutes to 5 hours. The appropriate treatment time can dissolve the fine fibers on the surface without damaging the fibers themselves, thereby maximizing the hydrogen bond density and bonding strength on the fiber surface.
[0019] Preferably, the second intermediate obtained after treatment with the treatment solution B needs to be left to stand for 1 to 24 hours.
[0020] Preferably, the drying method includes air drying at room temperature or oven drying at a drying temperature of 20 to 120°C; the cleaning solution is one or more of water, anhydrous ethanol, acetone, and toluene. The immersion treatment can effectively achieve the regeneration of cellulose on the fiber surface, thereby forming a dense structure.
[0021] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the super-strong bamboo material has excellent mechanical properties, the two-step treatment of natural bamboo material by solution A and solution B has a synergistic effect on the strength improvement of bamboo material, the tensile strength can reach nearly 1600MPa, and super-strong bamboo materials of different sizes can be prepared according to demand, which has broad application prospects. The present invention realizes self-reinforcement without adding any other substances by regulating the internal structure of natural bamboo material, fully exposes the fiber surface by delignification, and realizes close bonding between fibers and between fiber bundles by dissolving the fine fibers on the surface of large fibers, thereby improving the mechanical properties of bamboo material. It is a completely environmentally friendly, biodegradable and high-strength material. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1This is a scanning electron microscope cross-sectional morphology image between fiber bundles of the super-strong bamboo material prepared in Example 1;
[0023] Figure 2 This is a scanning electron microscope cross-sectional morphology of the fibers of the super-strong bamboo material prepared in Example 1;
[0024] Figure 3 This is a tensile stress-strain curve of the super-strong bamboo material prepared in Example 1. DETAILED DESCRIPTION
[0025] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0026] Example 1
[0027] like Figure 1 and Figure 2 As shown, a super-strong bamboo material includes delignified bamboo fibers and in-situ regenerated bamboo fibers. The bamboo fibers are exposed to more binding sites after delignification, and the pores of the bamboo fibers are tightly filled and tightly combined with the in-situ regenerated bamboo fibers to form a dense microstructure.
[0028] The preparation method of the above-mentioned super-strong bamboo material is as follows:
[0029] (1) immersing natural bamboo in a 2.5M sodium hydroxide / 0.5M sodium sulfite aqueous solution, wherein the mass ratio of the natural bamboo to the sodium hydroxide / sodium sulfite mixed solution is 1:10, heating at 95° C. for 2 h, then placing in a 10wt% hydrogen peroxide solution at 50° C. for 2 h, and washing with clean water to obtain a first intermediate;
[0030] (2) The above-mentioned partially delignined bamboo is immersed in a NN dimethylacetamide solution, the mass ratio of the absolute dry mass of the bamboo after delignification to the NN dimethylacetamide solution is 5:50, and it is placed in a 160°C environment for full reaction for 2 hours, then cooled to 105°C, lithium chloride is added for insulation treatment for 1 hour, the mass ratio of lithium chloride to the NN dimethylacetamide solution is 1:10, and it is allowed to stand for 5 hours to obtain a second intermediate;
[0031] (3) The second intermediate is washed with toluene and dried in an oven at 50° C. for 12 h to obtain the super-strong bamboo material.
[0032] The thickness of the obtained super-strong bamboo is 300μm, the tensile strength along the grain of the super-strong bamboo reaches 1568MPa, and the density is 1.56g / cm 3 , the thickness is reduced by 50% compared with natural bamboo, and the tensile strength along the grain is increased by about 4.2 times. For the tensile stress-strain curve, see Figure 3 .
[0033] Example 2
[0034] (1) immersing natural bamboo in a 2M sodium hydroxide aqueous solution, wherein the mass ratio of the natural bamboo material to the sodium hydroxide solution is 5:10, heating at 60° C. for 10 h, then placing in a 30 wt % hydrogen peroxide solution at 60° C. for 1 h, and washing with water to obtain a first intermediate;
[0035] (2) immersing the above-mentioned partially delignined bamboo material in a 1-methyl-3-methylimidazolium hydrochloride ion solution, wherein the mass ratio of the absolute dry mass of the delignified bamboo material to the 1-methyl-3-methylimidazolium hydrochloride ion solution is 3:50, and placing the bamboo material in a 90° C. environment to fully react for 4 hours to obtain a second intermediate;
[0036] (3) The second intermediate is washed with anhydrous ethanol and dried in an oven at 80°C for 6 h to obtain the super-strong bamboo material.
[0037] The thickness of the obtained super-strong bamboo is 500μm, the tensile strength along the grain of the super-strong bamboo reaches 680MPa, and the density is 1.25g / cm 3 The thickness is reduced by 16.7% compared with natural bamboo, and the tensile strength along the grain is increased by about 1.8 times.
[0038] Example 3
[0039] (1) immersing natural bamboo in a 30 wt % hydrogen peroxide solution, wherein the mass ratio of the hydrogen peroxide solution to the absolute dry mass of the natural bamboo is 3:10, heating at 50° C. for 12 h, and washing with clean water to obtain a first intermediate;
[0040] (2) immersing the above-mentioned partially delignined bamboo material in a copper-ammonia solution, wherein the mass ratio of the absolute dry mass of the delignified bamboo material to the copper-ammonia solution is 2:50, and placing the material in an environment of 80° C. for full reaction for 2 hours to obtain a second intermediate;
[0041] (3) The second intermediate is washed with anhydrous ethanol and dried in an oven at 120° C. for 2 h to obtain the super-strong bamboo material.
[0042] The thickness of the obtained super-strong bamboo is 380μm, the tensile strength along the grain of the super-strong bamboo reaches 580MPa, and the density is 1.41g / cm 3 The thickness is reduced by 36.7% compared with natural bamboo, and the tensile strength along the grain is increased by about 1.6 times.
[0043] Example 4
[0044] (1) immersing natural yellow bamboo in a 7 wt % sodium hypochlorite solution, wherein the mass ratio of the natural bamboo to the sodium hypochlorite solution is 5:10, heating at 80° C. for 3 h, and washing with clean water to obtain a first intermediate;
[0045] (2) immersing the above-mentioned partially delignined bamboo material in an alkali / urea mixed solution, wherein the mass ratio of the absolute dry mass of the delignified bamboo material to the alkali / urea mixed solution is 4:50, and placing the bamboo material in a -20°C environment to fully react for 2 hours to obtain a second intermediate;
[0046] (3) The second intermediate is washed with clean water and dried in an oven at 120° C. for 2 h to obtain the super-strong bamboo material.
[0047] The thickness of the obtained super-strong bamboo is 180μm, the tensile strength along the grain of the super-strong bamboo reaches 480MPa, and the density is 1.45g / cm 3 The thickness is 70% less than that of natural bamboo, and the tensile strength along the grain is increased by about 1.3 times.
[0048] Example 5
[0049] (1) immersing natural yellow bamboo in an acetic acid solution / hydrogen peroxide solution, wherein the mass ratio of the natural bamboo to the acetic acid solution / hydrogen peroxide mixed solution is 4:10, heating at 20° C. for 2 h, and washing with clean water to obtain a first intermediate;
[0050] (2) The above-mentioned partially delignined bamboo is immersed in a NN dimethylacetamide solution, the mass ratio of the absolute dry mass of the bamboo after delignification to the NN dimethylacetamide solution is 2:50, and it is placed in a 160°C environment for full reaction for 2 hours, then cooled to 105°C, a certain amount of lithium chloride is added, and the heat treatment is carried out for 1 hour, the mass ratio of lithium chloride to the NN dimethylacetamide solution is 1:10, and it is allowed to stand for 12 hours to obtain a second intermediate;
[0051] (3) The second intermediate is washed with clean water and dried in an oven at 120° C. for 2 h to obtain the super-strong bamboo material.
[0052] The thickness of the obtained super-strong bamboo is 280μm, the tensile strength along the grain of the super-strong bamboo reaches 1080MPa, and the density is 1.51g / cm 3 The thickness is 54% less than that of natural bamboo, and the tensile strength along the grain is increased by about 3 times.
[0053] Example 6
[0054] (1) immersing natural green bamboo in a 30 wt % hydrogen peroxide solution, wherein the mass ratio of the natural green bamboo to the hydrogen peroxide solution is 2:10, heating at 60° C. for 2 h, and washing with clean water to obtain a first intermediate;
[0055] (2) The above-mentioned partially delignined bamboo is immersed in a NN dimethylacetamide solution, the mass ratio of the absolute dry mass of the delignified bamboo to the NN dimethylacetamide solution is 3:50, and it is placed in a 160°C environment for full reaction for 2 hours, then cooled to 105°C, a certain amount of lithium chloride is added, and the heat treatment is carried out for 1 hour, the mass ratio of lithium chloride to the NN dimethylacetamide solution is 1:10, and it is allowed to stand for 12 hours to obtain a second intermediate;
[0056] (3) The second intermediate is washed with clean water and dried in an oven at 120° C. for 2 h to obtain the super-strong bamboo material.
[0057] The thickness of the obtained super-strong bamboo is 350μm, the tensile strength along the grain of the super-strong bamboo reaches 610MPa, and the density is 1.39g / cm 3 The thickness is 41% less than that of natural bamboo, and the tensile strength along the grain is increased by about 1.7 times.
[0058] Example 7
[0059] (1) immersing natural green bamboo in an acetic acid solution / hydrogen peroxide solution, wherein the mass ratio of the natural green bamboo to the acetic acid solution / hydrogen peroxide mixed solution is 4:10, heating at 40° C. for 10 h, and washing with clean water to obtain a first intermediate;
[0060] (2) immersing the above-mentioned partially delignined bamboo material in a copper-ammonia solution, wherein the mass ratio of the absolute dry mass of the delignified bamboo material to the copper-ammonia solution is 1:50, and placing the bamboo material in a 60° C. environment to fully react for 4 hours to obtain a second intermediate;
[0061] (3) The second intermediate is washed with anhydrous ethanol and dried in an oven at 40° C. for 20 h to obtain the super-strong bamboo material.
[0062] The thickness of the obtained super-strong bamboo is 230μm, the tensile strength along the grain of the super-strong bamboo reaches 540MPa, and the density is 1.48g / cm 3 The thickness is 61% less than that of natural bamboo, and the tensile strength along the grain is increased by about 1.5 times.
[0063] Example 8
[0064] (1) immersing natural green bamboo in a 10 wt % sodium hypochlorite solution, wherein the mass ratio of the natural green bamboo to the sodium hypochlorite solution is 3:10, heating at 60° C. for 1 h, and washing with clean water to obtain a first intermediate;
[0065] (2) placing the above-mentioned partially delignined bamboo material in an alkali / urea mixed solution, with the mass ratio of the absolute dry mass of the delignified bamboo material to the copper ammonia solution being 1:50, and placing it in a -50°C environment for full reaction for 5 hours to obtain a second intermediate;
[0066] (3) The second intermediate is washed with clean water and placed in an oven at 30° C. for 24 h to obtain the super-strong bamboo material.
[0067] The thickness of the obtained super-strong bamboo is 280μm, the tensile strength along the grain of the super-strong bamboo reaches 610MPa, and the density is 1.52g / cm 3 The thickness is 53% less than that of natural bamboo, and the tensile strength along the grain is increased by about 1.69 times.
Claims
1. A super strong bamboo material, It is characterized in that The super-strong bamboo material is a dense structure composed of micron-grade bamboo fibers and in-situ regenerated fibers, and the in-situ regenerated fibers are evenly distributed between single bamboo fibers and fiber bundles.
2. According to the super strong bamboo material of claim 1, It is characterized in that The longitudinal tensile strength of the super-strong bamboo material is 1300-1700 MPa, and the transverse tensile strength is 400-800 MPa.
3. According to the super strong bamboo material of claim 1, It is characterized in that The thickness of the super-strong bamboo material is 50-300 μm, and the density is 1.4-2.0 g·cm -3 .
4. A method for preparing the super-strong bamboo material according to any one of claims 1 to 3, It is characterized in that The following steps are involved: The natural bamboo material is immersed in a treatment solution A, delignified and washed to obtain a first intermediate; the treatment solution A is one or more of a strong alkaline solution, an acetic acid solution, a hydrogen peroxide solution, a sodium hypochlorite solution, and a sodium sulfite solution; The first intermediate is immersed in a treatment solution B to dissolve part of the fiber to obtain a second intermediate; the treatment solution B is one or more of an alkali / urea mixed solution, a lithium chloride / NN dimethylacetamide solution, an N-methylmorpholine-N-oxide solution, an ion solution, and a cuprammonia solution; The second intermediate is washed and dried to obtain super strong bamboo.
5. The method for preparing the super-strong bamboo material according to claim 4, It is characterized in that The natural bamboo material is derived from yellow bamboo, nan bamboo, green bamboo or bitter bamboo.
6. The method for preparing the super-strong bamboo material according to claim 4, It is characterized in that The mass ratio of the absolute dry mass of the natural bamboo material to the A treatment solution is 1-5:10, and the delignification treatment method comprises: soaking in the A treatment solution at 50-100° C. for 1-12 hours, and washing with water after delignification.
7. The method for preparing the super-strong bamboo material according to claim 4, It is characterized in that The mass ratio of the absolute dry mass of the delignified bamboo to the mass of the B treatment solution is 1:5-50.
8. The method for preparing the super-strong bamboo material according to claim 4, It is characterized in that The treatment temperature of the B treatment solution is -50 to 200° C., and the treatment time is 10 min to 5 h.
9. The method for preparing the super-strong bamboo material according to claim 4, It is characterized in that The second intermediate obtained after treatment with solution B needs to be left to stand for 1 to 24 hours.
10. The method for preparing the super-strong bamboo material according to claim 4, It is characterized in that The drying method includes air drying at room temperature or oven drying, with the drying temperature being 20-120°C.