Photomask substrate processing method

By using diamond grinding wheels with different precision for grinding and polishing, the problem of high planeness and parallelism requirements for large-size photomask substrates is solved, and an efficient and low-cost processing process is achieved, and no traces of the tool and steps are obtained. uniform surface.

CN118990829APending Publication Date: 2024-11-22HUNAN OMNISUN INFORMATION MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410948970.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the case of large size, the existing photomask substrate processing methods have high requirements for raw material thickness, planarity and parallelism, complex process and low economical utility, and long processing time.

Method used

Diamond grinding wheels with different precision are grinding in sequence, and they are reciprocating in the X-axis direction. The diamond grinding wheel is continuously fed along the Y-axis to gradually improve the flatness of the glass substrate and remove the damaged layer. Combined with spray cleaning and polishing technology, the tool-free is achieved A uniform matte surface of traces and steps.

Benefits of technology

The process flow is simplified, processing efficiency and economical effectiveness are improved, production costs are reduced, and high-precision needs of large-size photomask substrates are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118990829A_ABST
    Figure CN118990829A_ABST
Patent Text Reader

Abstract

The invention discloses a photomask substrate processing method, which is characterized in that a photomask substrate raw material is a glass substrate, and the processing method comprises the following steps: carrying out edge grinding, edge grinding, chamfering and spray cleaning on the glass substrate to obtain measurement data for glass substrate processing, determining a processing scheme according to the measurement data, diamond grinding wheels with different accuracies are used for grinding with different accuracies in sequence; after grinding, sequentially carrying out rough polishing and fine polishing on the glass substrate by using polishing equipment, sequentially carrying out grinding with different precisions by using diamond grinding wheels with different precisions, and gradually removing a damaged layer on the surface of the glass substrate after the previous grinding while rapidly improving the flatness of the raw material; the diamond grinding wheel continuously feeds along the Y axis, the advancing track of the glass substrate is similar to a W shape, the uniform frosted surface without feeding traces and steps can be obtained after grinding, the requirement for raw materials is not high, the technological process is simple and convenient, the machining efficiency is high, the production cost is low, and the economic effectiveness is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a photomask substrate, and in particular to a photomask substrate processing method. Background Art

[0002] The mask, also known as the photomask, is a master template for pattern transfer in the microelectronics manufacturing process and is widely used in the fields of semiconductors, flat panel displays, printed circuit boards, etc. The function of the mask is similar to the "negative" of a traditional camera. Its role is to transfer the designed circuit pattern to the photoresist film on the wafer or quartz substrate through processes such as photolithography, development, and etching in cooperation with the photolithography machine and photoresist, so as to replicate the circuit pattern and realize mass production.

[0003] According to the different downstream application industries, the mask can be divided into panel mask, semiconductor mask, touch mask and circuit board mask. Panel mask can be used in thin film transistor liquid crystal display TFT-LCD, AMOLED, fine metal mask FMM and other fields. Panel mask is evolving in two directions: large size and high precision. On the one hand, benefiting from the increasing screen size of consumer electronic products such as flat-panel TVs, smart phones, and computers, the development of the global flat panel display industry has shown a large size, and the mask size has also been correspondingly large, which has posed a higher challenge to the manufacture of mask. On the other hand, in order to meet the increasing requirements of consumers for display products, flat panel displays are being driven towards higher definition and high color saturation. Research institutions predict that the display accuracy of future display screens will gradually increase from 450PPI (pixels per inch) to more than 650PPI. The continuous increase in the number of pixels per inch will also bring about an increase in the requirements for parameters such as lithography resolution, CD uniformity, defect size, and overlay accuracy of flat panel display masks.

[0004] The most important raw material in the mask is the mask substrate. As the carrier of the mask pattern, the mask substrate plays an important role in the precision and quality of the mask product. The substrate must have good optical transmittance, size and chemical stability, flatness, etc., and no tiny defects such as sand inclusions and bubbles. Due to the stable chemical properties, high optical transmittance and low thermal expansion coefficient of quartz glass, it has become the mainstream raw material for preparing masks in recent years. For large-sized mask substrates, surface flatness and tiny defects are the key factors determining their precision. If the flatness of a large-sized mask substrate is low, when the light is directly irradiated, it will cause the light to deflect relative to the ideal plane, the size of the lithography pattern will change (enlarge or reduce), and the lithography resolution will be reduced. Therefore, ensuring the high flatness of the mask substrate is the basic prerequisite for obtaining high precision.

[0005] The existing large-size photomask substrate flatness processing method adopts at least one method of grinding, grinding and polishing to achieve the flatness of the photomask substrate. The main purpose is to obtain a high-flatness photomask substrate to improve the photolithography resolution.

[0006] Invention patent CN1437045A-Large size substrate and its manufacturing method discloses a large size substrate having a diagonal length of not less than 500mm and a flatness / diagonal length ratio of not more than 6.0×10-6. This method first performs double-sided grinding on the raw material plate to pre-make the parallelism reach 50um or even below 10um, otherwise the subsequent processing will cause thicker parts of the plate to be removed, resulting in long processing time and excessive plate thickness removal. Afterwards, the high points on the surface of the plate are locally processed by controlling the processing parameters of the sandblaster. This method has high requirements on the parallelism of the raw materials, and the sandblasting process is relatively complicated, and has high requirements on the operators and processing equipment, resulting in certain restrictions on its application.

[0007] Invention patent CN101246312-Recycling of large-size photomask substrates discloses a method for recycling used large-size photomask substrates with patterned light-shielding films. The method uses a sandblasting + polishing process to prepare a reused photomask substrate. However, the method requires the raw material thickness to be at least 3mm, and the surface of the glass substrate is also resurfaced through a complex sandblasting process.

[0008] Invention patent CN101804589A-Method for processing artificial quartz glass substrate for semiconductors discloses a method for processing artificial quartz glass substrate for semiconductors using a small rotary polishing component. The method requires that the surface flatness of the substrate to be polished should be at least 2um before polishing. Moreover, when the area of ​​the glass substrate to be processed is greater than 1×105mm2 (about 223.6mm on the diagonal), the contact area of ​​the small rotary tool is too small relative to the substrate, resulting in a very long processing time. Summary of the invention

[0009] In view of the existing photomask substrate processing methods, when the size of the photomask substrate is large, there are high restrictions on the thickness, flatness, parallelism, etc. of the raw materials, the process flow is relatively complicated, the processing time is long, and the economic benefits are low. The present invention provides a photomask substrate processing method, which uses diamond grinding wheels with different precisions to perform grinding with different precisions in sequence, while quickly improving the flatness of the raw material, and gradually removing the damaged layer on the surface of the glass substrate after the last grinding. When the raw material reciprocates along the X-axis direction, the diamond grinding wheel continuously feeds along the Y-axis, and the travel trajectory of the glass substrate is similar to a W-shape. After grinding, a uniform frosted surface without tool traces and steps can be obtained.

[0010] To achieve the above object, the embodiments of the present invention adopt the following technical solutions:

[0011] A photomask substrate processing method, wherein the raw material of the photomask substrate is a glass substrate, and the processing method comprises:

[0012] Performing preliminary processing on the glass substrate;

[0013] Spray cleaning the glass substrate;

[0014] Obtaining measurement data for glass substrate processing and determining a processing plan based on the measurement data;

[0015] The glass substrate is processed according to the processing plan.

[0016] According to one aspect of the present invention, the edge grinding, edge grinding and chamfering of the glass substrate comprises: placing the glass substrate flat on a rubber vacuum suction cup of a precision engraving machine to perform edge grinding, edge grinding and chamfering processes.

[0017] According to one aspect of the present invention, the spray cleaning of the glass substrate comprises: placing the glass substrate in a water tank, spray cleaning the front and back surfaces of the glass substrate, and after spray cleaning, using clean compressed air to blow dry water marks on the front and back surfaces of the glass substrate.

[0018] According to one aspect of the present invention, the measuring of basic data of the glass substrate includes: using a flatness image tester to measure the flatness, parallelism, thickness and surface shape of the glass substrate, and calculating the total feed amount of the grinding process according to the surface shape of the glass substrate.

[0019] According to one aspect of the present invention, the processing scheme comprises:

[0020] The surface with poor flatness is selected as the front surface, and the other surface is selected as the back surface, and the front surface is the first surface to be processed;

[0021] Grinding a glass substrate;

[0022] The glass substrate is polished.

[0023] According to one aspect of the present invention, the grinding process of the glass substrate includes: placing the glass substrate flat on the magnetic worktable of the surface grinder, using precision gap gauges of different thicknesses to measure the adjacent gap between the raw material glass substrate and the worktable, filling and adjusting the gap by using a precision gap gauge of appropriate thickness, selecting diamond grinding wheels with different particle sizes to perform rough grinding, semi-finishing grinding, and fine grinding on the glass substrate in sequence, and spray cleaning the glass substrate after each grinding.

[0024] According to one aspect of the present invention, the rough grinding method includes: using a diamond grinding wheel with a particle size of 270# for rough grinding, the glass substrate reciprocates along the X-axis direction, the diamond grinding wheel continuously feeds along the Y-axis direction, after reciprocating once in the Y-axis direction, the diamond grinding wheel intermittently feeds once again along the Z-axis direction perpendicular to the front side of the glass substrate, after the front side of the glass substrate is roughly ground and spray-cleaned, the back side of the glass substrate is roughly ground and spray-cleaned, and the surface flatness of the glass substrate after grinding is measured.

[0025] According to one aspect of the present invention, the semi-finishing grinding method includes: using a diamond grinding wheel with a particle size of 500# for semi-finishing grinding, the glass substrate reciprocates along the X-axis direction, the diamond grinding wheel continuously feeds along the Y-axis direction, after reciprocating once in the Y-axis direction, the diamond grinding wheel intermittently feeds once again along the Z-axis direction perpendicular to the front side of the glass substrate, after semi-finishing grinding and spray cleaning of the front side of the glass substrate, semi-finishing grinding and spray cleaning of the back side of the glass substrate are performed, and the surface flatness of the glass substrate after grinding is measured.

[0026] According to one aspect of the present invention, the fine grinding method includes: using a diamond grinding wheel with a particle size of 800#-1340# for fine grinding, the glass substrate reciprocates along the X-axis direction, the diamond grinding wheel continuously feeds along the Y-axis direction, after reciprocating once in the Y-axis direction, the diamond grinding wheel intermittently feeds once again along the Z-axis direction perpendicular to the front side of the glass substrate, after fine grinding and spray cleaning the front side of the glass substrate, fine grinding and spray cleaning the back side of the glass substrate, and measuring the surface flatness of the glass substrate after grinding.

[0027] According to one aspect of the present invention, the polishing process of the glass substrate includes: sequentially performing rough polishing and fine polishing on the glass substrate; the rough polishing includes: after grinding, using a polishing device to perform chemical mechanical polishing on the raw material glass substrate, the glass substrate is placed flat in a star tray, the upper and lower surfaces thereof are in contact with a rough polishing pad, and a polishing powder with a particle size of 1um-5um is selected; the fine polishing includes: after grinding, using a polishing device to perform chemical mechanical polishing on the raw material glass substrate, the glass substrate is placed flat in a star tray, the upper and lower surfaces thereof are in contact with a rough polishing pad, and a polishing powder with a particle size of 0.5um-3um is selected.

[0028] Advantages of the implementation of the present invention: The present invention provides a method for processing a photomask substrate, wherein the raw material of the photomask substrate is a glass substrate, and the processing method comprises: grinding the edges, chamfering, and spray cleaning the glass substrate, obtaining measurement data for glass substrate processing, determining a processing plan according to the measurement data, and using diamond grinding wheels of different precisions to perform grinding of different precisions in sequence; after grinding, using a polishing device to perform rough polishing and fine polishing on the glass substrate in sequence, and using diamond grinding wheels of different precisions to perform grinding of different precisions in sequence, while quickly improving the flatness of the raw material, gradually removing the damaged layer on the surface of the glass substrate after the last grinding, and when the raw material reciprocates along the X-axis direction, the diamond grinding wheel continuously feeds along the Y-axis, and the travel trajectory of the glass substrate is similar to a W-shape, and a uniform frosted surface without tool traces and steps can be obtained after grinding, and the requirements for raw materials are not high, the process flow is simple, the processing efficiency is high, the production cost is low, and the economic benefit is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 The present invention is a flowchart of a photomask substrate processing method. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] like Figure 1 As shown, a photomask substrate processing method, the raw material of the photomask substrate is a synthetic quartz glass substrate, the size of which is 450×550 mm (diagonal length 711 mm) and the thickness is 5.0 mm, and the processing method includes:

[0034] Step S1: performing preliminary processing on the glass substrate;

[0035] Place the glass substrate flat on the rubber vacuum suction cup of the engraving machine for edge grinding, edge grinding and chamfering.

[0036] Step S2: spray cleaning the glass substrate;

[0037] Place the glass substrate in a water tank, spray clean the front and back of the glass substrate, and after spray cleaning, use clean compressed air to blow dry the water marks on the front and back of the glass substrate.

[0038] Step S3: obtaining measurement data for glass substrate processing, and determining a processing plan based on the measurement data;

[0039] Use a flatness image tester to measure the flatness, parallelism, thickness and surface shape of the glass substrate, and calculate the total feed amount of the rough grinding process.

[0040] Processing solutions include:

[0041] The surface with poor flatness is selected as the front surface, and the other surface is selected as the back surface, and the front surface is the first surface to be processed;

[0042] Grinding a glass substrate;

[0043] The glass substrate is polished.

[0044] In this embodiment, the original glass substrate has a flatness of 28um for surface A, 46um for surface B, a parallelism of 15um, and a thickness of 5.062mm. Surface B with poor flatness is used as the front surface, and the surface shape of the surface is convex, that is, the middle area is high and the four side areas are low.

[0045] In practical applications, flatness, parallelism, and thickness measurements are performed using a set of high-precision KEYENCE laser transmitters to emit visible red lasers to the surface of the object being measured. The laser reflected by the object is received by the internal CCD linear camera through the receiver lens. Depending on the distance, the CCD linear camera can receive the light spot at different angles. Based on this, the digital signal processor can calculate the thickness of the glass substrate to be measured, and at the same time obtain the surface point cloud data of the glass substrate to be measured, and then obtain the flatness and parallelism of the glass substrate to be measured through the software algorithm.

[0046] Step S4: processing the glass substrate according to the processing plan;

[0047] Place the glass substrate flat on the magnetic work surface of the surface grinder, use precision gap gauges with thicknesses of 10um, 20um, and 50um to measure the adjacent gap between the raw material glass substrate and the work surface, and fill and adjust the gap using a precision gap gauge of appropriate thickness.

[0048] The grinding process of the glass substrate includes: selecting diamond grinding wheels with different particle sizes to sequentially perform rough grinding, semi-finishing grinding and fine grinding on the glass substrate, and spray cleaning the glass substrate after each grinding.

[0049] The polishing process for the glass substrate includes: sequentially performing rough polishing and fine polishing on the glass substrate.

[0050] In practical applications, when the gap is large, a precision gap ruler of appropriate thickness can be used to fill the gap between the glass substrate and the work surface.

[0051] Step S41: performing rough grinding on the glass substrate;

[0052] A 270# diamond grinding wheel was used for rough grinding. The 270# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 300mm / min. After one reciprocating motion in the Y-axis direction, the 270# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 10um and the total feed amount was 50um. After the grinding procedure was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate, and the measured flatness was 12.9um.

[0053] Then turn the glass over and grind the A side. The 270# diamond grinding wheel continuously feeds along the Y axis at a rate of 300mm / min. The 270# diamond grinding wheel feeds 10um in a single time along the Z axis, and the total feed is 30um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the flatness of the surface of the ground glass substrate, and the flatness is measured to be 13.3um.

[0054] Step S42: performing semi-finishing grinding on the glass substrate;

[0055] A 500# diamond grinding wheel was used for semi-finishing grinding. The 500# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 300mm / min. After one reciprocating motion in the Y-axis direction, the 500# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 5um and the total feed amount was 20um. After the grinding procedure was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0056] Then turn the glass over and grind the A side. The 500# diamond grinding wheel continuously feeds along the Y-axis at a rate of 300mm / min, and the 500# diamond grinding wheel feeds 5um at a single time along the Z-axis, with a total feed of 20um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the surface flatness of the ground glass substrate.

[0057] Step S43: performing fine grinding on the glass substrate;

[0058] A diamond grinding wheel with a particle size of 800# was used for fine grinding. The 800# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 300mm / min. After one reciprocating motion in the Y-axis direction, the 800# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 3um and the total feed amount was 10um. After the grinding program was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0059] Then turn the glass over and grind the A side. The 800# diamond grinding wheel continuously feeds along the Y-axis at a rate of 300mm / min, and the 800# diamond grinding wheel feeds 3um at a single time along the Z-axis, with a total feed of 10um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the surface flatness of the ground glass substrate.

[0060] A 1340# diamond grinding wheel was used for fine grinding. The 1340# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 300mm / min. After one reciprocating motion in the Y-axis direction, the 1340# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 1um and the total feed amount was 5um. After the grinding program was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0061] The glass was turned over and the A side was ground. The 1340# diamond grinding wheel continuously fed along the Y-axis at a rate of 300mm / min. The 1340# diamond grinding wheel fed along the Z-axis with a single feed of 1um and a total feed of 5um. After the grinding process was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate. The front flatness was measured to be 7.1um and the back flatness was 6.1um.

[0062] Step S44: performing rough polishing on the glass substrate;

[0063] After grinding, the raw material glass substrate is chemically mechanically polished using a polishing device. The glass substrate is placed flat in the star tray, with its upper and lower surfaces in contact with the rough polishing pad, and a polishing powder with a particle size of 1um-5um is selected;

[0064] Step S45: performing fine polishing on the glass substrate;

[0065] Fine polishing includes: after grinding, the raw material glass substrate is chemically and mechanically polished using a polishing device, the glass substrate is placed flat in the star tray, its upper and lower surfaces are in contact with the rough polishing pad, and a polishing powder with a particle size of 0.5um-3um is selected;

[0066] After mechanical polishing, the flatness of the glass substrate was measured using a flatness image tester and was found to be 4.8um and 4.2um.

[0067] In practical applications, the polishing powder is mainly cerium dioxide, and the concentration of the polishing powder suspended in water is 5wt%-15wt%.

[0068] Example 2

[0069] The raw material of the photomask substrate is a synthetic quartz glass substrate with a size of 420×520 mm (diagonal length 668 mm) and a thickness of 5.0 mm. The processing method includes:

[0070] Step S1: performing preliminary processing on the glass substrate;

[0071] Place the glass substrate flat on the rubber vacuum suction cup of the engraving machine for edge grinding, edge grinding and chamfering.

[0072] Step S2: spray cleaning the glass substrate;

[0073] Place the glass substrate in a water tank, spray clean the front and back of the glass substrate, and after spray cleaning, use clean compressed air to blow dry the water marks on the front and back of the glass substrate.

[0074] Step S3: obtaining measurement data for glass substrate processing, and determining a processing plan based on the measurement data;

[0075] Use a flatness image tester to measure the flatness, parallelism, thickness and surface shape of the glass substrate, and calculate the total feed amount of the rough grinding process.

[0076] Processing solutions include:

[0077] The surface with poor flatness is selected as the front surface, and the other surface is selected as the back surface, and the front surface is the first surface to be processed;

[0078] Grinding a glass substrate;

[0079] The glass substrate is polished.

[0080] In this embodiment, the original glass substrate has a flatness of 52 um for surface A, 32 um for surface B, a parallelism of 11 um, and a thickness of 4.821 mm. Surface A with poor flatness is used as the front surface.

[0081] Step S4: processing the glass substrate according to the processing plan;

[0082] Place the glass substrate flat on the magnetic work surface of the surface grinder, use precision gap gauges with thicknesses of 10um, 20um, and 50um to measure the adjacent gap between the raw material glass substrate and the work surface, and fill and adjust the gap using a precision gap gauge of appropriate thickness.

[0083] The grinding process of the glass substrate includes: selecting diamond grinding wheels with different particle sizes to sequentially perform rough grinding, semi-finishing grinding and fine grinding on the glass substrate, and spray cleaning the glass substrate after each grinding.

[0084] The polishing process for the glass substrate includes: sequentially performing rough polishing and fine polishing on the glass substrate.

[0085] Step S41: performing rough grinding on the glass substrate;

[0086] A 270# diamond grinding wheel was used for rough grinding. The 270# diamond grinding wheel continuously fed along the Y-axis at a rate of 300mm / min. After one reciprocating motion in the Y-axis direction, the 270# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 10um and the total feed amount was 50um. After the grinding procedure was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0087] Then turn the glass over and grind the A side. The 270# diamond grinding wheel continuously feeds along the Y axis at a rate of 300mm / min. The 270# diamond grinding wheel feeds 10um in a single time along the Z axis, and the total feed is 30um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the flatness of the surface of the ground glass substrate.

[0088] Step S42: performing semi-finishing grinding on the glass substrate;

[0089] A 500# diamond grinding wheel was used for semi-finishing grinding. The 500# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 300mm / min. After one reciprocating motion in the Y-axis direction, the 500# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 5um and the total feed amount was 20um. After the grinding procedure was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0090] Then turn the glass over and grind the A side. The 500# diamond grinding wheel continuously feeds along the Y-axis at a rate of 300mm / min, and the 500# diamond grinding wheel feeds 5um at a single time along the Z-axis, with a total feed of 20um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the surface flatness of the ground glass substrate.

[0091] Step S43: performing fine grinding on the glass substrate;

[0092] A diamond grinding wheel with a particle size of 800# was used for fine grinding. The 800# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 300mm / min. After one reciprocating motion in the Y-axis direction, the 800# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 3um and the total feed amount was 10um. After the grinding program was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0093] Then turn the glass over and grind the A side. The 800# diamond grinding wheel continuously feeds along the Y-axis at a rate of 300mm / min, and the 800# diamond grinding wheel feeds 3um at a single time along the Z-axis, with a total feed of 10um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the surface flatness of the ground glass substrate.

[0094] A 1340# diamond grinding wheel was used for fine grinding. The 1340# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 300mm / min. After one reciprocating motion in the Y-axis direction, the 1340# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 1um and the total feed amount was 5um. After the grinding program was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0095] Then turn the glass over and grind the A side. The 1340# diamond grinding wheel continuously feeds along the Y-axis at a rate of 300mm / min. The 1340# diamond grinding wheel feeds 1um at a single time along the Z-axis, and the total feed is 5um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the surface flatness of the ground glass substrate.

[0096] Step S44: performing rough polishing on the glass substrate;

[0097] Rough polishing includes: after grinding, the raw material glass substrate is chemically mechanically polished using a polishing device, the glass substrate is placed flat in the star tray, and its upper and lower surfaces are in contact with the rough polishing pad, and a polishing powder with a particle size of 1um-5um is selected;

[0098] Step S45: performing fine polishing on the glass substrate;

[0099] Fine polishing includes: after grinding, the raw material glass substrate is chemically and mechanically polished using a polishing device, the glass substrate is placed flat in the star tray, its upper and lower surfaces are in contact with the rough polishing pad, and a polishing powder with a particle size of 0.5um-3um is selected;

[0100] After mechanical polishing, the flatness of the glass substrate was measured using a flatness image tester and was found to be 7.4um and 5.8um.

[0101] Example 3

[0102] The raw material of the photomask substrate is a synthetic quartz glass substrate with a size of 520×800 mm (diagonal length 954 mm) and a thickness of 9.8 mm. The processing method includes:

[0103] Step 1: Preliminary treatment of the glass substrate;

[0104] Place the glass substrate flat on the rubber vacuum suction cup of the engraving machine for edge grinding, edge grinding and chamfering.

[0105] Step S2: spray cleaning the glass substrate;

[0106] Place the glass substrate in a water tank, spray clean the front and back of the glass substrate, and after spray cleaning, use clean compressed air to blow dry the water marks on the front and back of the glass substrate.

[0107] Step S3: obtaining measurement data for glass substrate processing, and determining a processing plan based on the measurement data;

[0108] Use a flatness image tester to measure the flatness, parallelism, thickness and surface shape of the glass substrate, and calculate the total feed amount of the rough grinding process.

[0109] Processing solutions include:

[0110] The surface with poor flatness is selected as the front surface, and the other surface is selected as the back surface, and the front surface is the first surface to be processed;

[0111] Grinding a glass substrate;

[0112] The glass substrate is polished.

[0113] In this embodiment, the original glass substrate has a flatness of 89 um for surface A, 63 um for surface B, a parallelism of 51 um, and a thickness of 9.807 mm. Surface A with poor flatness is used as the front surface.

[0114] Step S4: processing the glass substrate according to the processing plan;

[0115] Place the glass substrate flat on the magnetic work surface of the surface grinder, use precision gap gauges with thicknesses of 10um, 20um, and 50um to measure the adjacent gap between the raw material glass substrate and the work surface, and fill and adjust the gap using a precision gap gauge of appropriate thickness.

[0116] The grinding process of the glass substrate includes: selecting diamond grinding wheels with different particle sizes to sequentially perform rough grinding, semi-finishing grinding and fine grinding on the glass substrate, and spray cleaning the glass substrate after each grinding.

[0117] The polishing process of the glass substrate includes: performing rough polishing and fine polishing on the glass substrate in sequence.

[0118] Step S41: performing rough grinding on the glass substrate;

[0119] A 270# diamond grinding wheel was used for rough grinding. The 270# diamond grinding wheel continuously fed along the Y-axis at a rate of 400mm / min. After one reciprocating motion in the Y-axis direction, the 270# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 10um and the total feed amount was 260um. After the grinding procedure was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate, and the measured flatness was 12.3um.

[0120] Then turn the glass over and grind the A side. The 270# diamond grinding wheel continuously feeds along the Y axis at a rate of 400mm / min. The 270# diamond grinding wheel feeds 10um in a single time along the Z axis, and the total feed is 110um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the flatness of the surface of the ground glass substrate, and the flatness is measured to be 13.7um.

[0121] Step S42: performing semi-finishing grinding on the glass substrate;

[0122] A 500# diamond grinding wheel was used for semi-finishing grinding. The 500# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 400mm / min. After one reciprocating motion in the Y-axis direction, the 500# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 5um and the total feed amount was 30um. After the grinding procedure was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0123] Then turn the glass over and grind the A side. The 500# diamond grinding wheel continuously feeds along the Y-axis at a rate of 400mm / min, and the 500# diamond grinding wheel feeds 5um at a single time along the Z-axis, with a total feed of 30um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the surface flatness of the ground glass substrate.

[0124] Step S43: performing fine grinding on the glass substrate;

[0125] A diamond grinding wheel with a particle size of 800# was used for fine grinding. The 800# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 400mm / min. After one reciprocating motion in the Y-axis direction, the 800# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 3um and the total feed amount was 10um. After the grinding program was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0126] Then turn the glass over and grind the A side. The 800# diamond grinding wheel continuously feeds along the Y-axis at a rate of 400mm / min, and the 800# diamond grinding wheel feeds 3um at a single time along the Z-axis, with a total feed of 10um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the surface flatness of the ground glass substrate.

[0127] A 1000# diamond grinding wheel was used for fine grinding. The 1000# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 400mm / min. After one reciprocating motion in the Y-axis direction, the 1000# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 1um and the total feed amount was 5um. After the grinding program was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0128] Then turn the glass over and grind the A side. The 1000# diamond grinding wheel continuously feeds along the Y-axis at a rate of 400mm / min, and the 1000# diamond grinding wheel feeds 1um at a single time along the Z-axis, with a total feed of 5um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the surface flatness of the ground glass substrate.

[0129] Step S44: performing rough polishing on the glass substrate;

[0130] Rough polishing includes: after grinding, the raw material glass substrate is chemically mechanically polished using a polishing device, the glass substrate is placed flat in the star tray, and its upper and lower surfaces are in contact with the rough polishing pad, and a polishing powder with a particle size of 1um-5um is selected;

[0131] Step S45: performing fine polishing on the glass substrate;

[0132] Fine polishing includes: after grinding, the raw material glass substrate is chemically and mechanically polished using a polishing device, the glass substrate is placed flat in the star tray, its upper and lower surfaces are in contact with the rough polishing pad, and a polishing powder with a particle size of 0.5um-3um is selected;

[0133] After mechanical polishing, the flatness of the glass substrate was measured using a flatness image tester and was found to be 7.1um and 6.1um.

[0134] Example 4

[0135] The raw material of the photomask substrate is a synthetic quartz glass substrate with a size of 800×960 mm (diagonal length 1250 mm) and a thickness of 9.8 mm. The processing method includes:

[0136] Step 1: Preliminary treatment of the glass substrate;

[0137] Place the glass substrate flat on the rubber vacuum suction cup of the engraving machine for edge grinding, edge grinding and chamfering.

[0138] Step S2: spray cleaning the glass substrate;

[0139] Place the glass substrate in a water tank, spray clean the front and back of the glass substrate, and after spray cleaning, use clean compressed air to blow dry the water marks on the front and back of the glass substrate.

[0140] Step S3: obtaining measurement data for glass substrate processing, and determining a processing plan based on the measurement data;

[0141] Use a flatness image tester to measure the flatness, parallelism, thickness and surface shape of the glass substrate, and calculate the total feed amount of the rough grinding process.

[0142] Processing solutions include:

[0143] The surface with poor flatness is selected as the front surface, and the other surface is selected as the back surface, and the front surface is the first surface to be processed;

[0144] Grinding a glass substrate;

[0145] The glass substrate is polished.

[0146] In this embodiment, the original glass substrate has a flatness of 250 um for surface A, 993 um for surface B, a parallelism of 67 um, and a thickness of 10.044 mm. Surface A with poor flatness is used as the front surface.

[0147] Step S4: processing the glass substrate according to the processing plan;

[0148] Place the glass substrate flat on the magnetic work surface of the surface grinder, use precision gap gauges with thicknesses of 10um, 20um, and 50um to measure the adjacent gap between the raw material glass substrate and the work surface, and fill and adjust the gap using a precision gap gauge of appropriate thickness.

[0149] The grinding process of the glass substrate includes: selecting diamond grinding wheels with different particle sizes to sequentially perform rough grinding, semi-finishing grinding and fine grinding on the glass substrate, and spray cleaning the glass substrate after each grinding.

[0150] The polishing process for the glass substrate includes: sequentially performing rough polishing and fine polishing on the glass substrate.

[0151] Step S41: performing rough grinding on the glass substrate;

[0152] A 270# diamond grinding wheel was used for rough grinding. The 270# diamond grinding wheel continuously fed along the Y-axis at a rate of 400mm / min. After one reciprocating motion in the Y-axis direction, the 270# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 10um and the total feed amount was 260um. After the grinding procedure was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate, and the measured flatness was 12.3um.

[0153] Then turn the glass over and grind the A side. The 270# diamond grinding wheel continuously feeds along the Y axis at a rate of 400mm / min. The 270# diamond grinding wheel feeds 10um in a single time along the Z axis, and the total feed is 110um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the flatness of the surface of the ground glass substrate, and the flatness is measured to be 13.7um.

[0154] Step S42: performing semi-finishing grinding on the glass substrate;

[0155] A 500# diamond grinding wheel was used for semi-finishing grinding. The 500# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 400mm / min. After one reciprocating motion in the Y-axis direction, the 500# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 5um and the total feed amount was 30um. After the grinding procedure was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0156] Then turn the glass over and grind the A side. The 500# diamond grinding wheel continuously feeds along the Y-axis at a rate of 400mm / min, and the 500# diamond grinding wheel feeds 5um at a single time along the Z-axis, with a total feed of 30um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the surface flatness of the ground glass substrate.

[0157] Step S43: performing fine grinding on the glass substrate;

[0158] A diamond grinding wheel with a particle size of 800# was used for fine grinding. The 800# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 400mm / min. After one reciprocating motion in the Y-axis direction, the 800# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 3um and the total feed amount was 10um. After the grinding program was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0159] Then turn the glass over and grind the A side. The 800# diamond grinding wheel continuously feeds along the Y-axis at a rate of 400mm / min, and the 800# diamond grinding wheel feeds 3um at a single time along the Z-axis, with a total feed of 10um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the surface flatness of the ground glass substrate.

[0160] A 1000# diamond grinding wheel was used for fine grinding. The 1000# diamond grinding wheel continuously fed along the Y-axis direction at a rate of 400mm / min. After one reciprocating motion in the Y-axis direction, the 1000# diamond grinding wheel intermittently fed once along the Z-axis direction perpendicular to the front of the glass substrate. The single feed amount was 1um and the total feed amount was 5um. After the grinding program was completed, the surface of the glass substrate was rinsed with pure water and then dried with clean compressed air. The VML7S ultra-precision electronic level was used to measure the surface flatness of the ground glass substrate.

[0161] Then turn the glass over and grind the A side. The 1000# diamond grinding wheel continuously feeds along the Y-axis at a rate of 400mm / min, and the 1000# diamond grinding wheel feeds 1um at a single time along the Z-axis, with a total feed of 5um. After the grinding process is completed, the surface of the glass substrate is rinsed with pure water and then blown dry with clean compressed air. The VML7S ultra-precision electronic level is used to measure the surface flatness of the ground glass substrate.

[0162] Step S44: performing rough polishing on the glass substrate;

[0163] Rough polishing includes: after grinding, the raw material glass substrate is chemically mechanically polished using a polishing device, the glass substrate is placed flat in the star tray, and its upper and lower surfaces are in contact with the rough polishing pad, and a polishing powder with a particle size of 1um-5um is selected;

[0164] Step S45: performing fine polishing on the glass substrate;

[0165] Fine polishing includes: after grinding, the raw material glass substrate is chemically and mechanically polished using a polishing device, the glass substrate is placed flat in the star tray, its upper and lower surfaces are in contact with the rough polishing pad, and a polishing powder with a particle size of 0.5um-3um is selected;

[0166] After mechanical polishing, the flatness of the glass substrate was measured using a flatness image tester and was found to be 12.0um and 8.9um.

[0167] Advantages of the implementation of the present invention: The present invention discloses a method for processing a photomask substrate, wherein the raw material of the photomask substrate is a glass substrate, and the processing method comprises: grinding the edges, chamfering, and spray cleaning the glass substrate, obtaining measurement data for glass substrate processing, determining a processing plan according to the measurement data, and using diamond grinding wheels of different precisions to perform grinding of different precisions in sequence; after grinding, using a polishing device to perform rough polishing and fine polishing on the glass substrate in sequence, and using diamond grinding wheels of different precisions to perform grinding of different precisions in sequence, while quickly improving the flatness of the raw material, gradually removing the damaged layer on the surface of the glass substrate after the last grinding, and when the raw material reciprocates along the X-axis direction, the diamond grinding wheel continuously feeds along the Y-axis, and the travel trajectory of the glass substrate is similar to a W-shape, and a uniform frosted surface without tool traces and steps can be obtained after grinding, and the requirements for raw materials are not high, the process flow is simple, the processing efficiency is high, the production cost is low, and the economic benefit is high.

[0168] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A method for processing a photomask substrate, wherein the raw material of the photomask substrate is a glass substrate, characterized in that: The processing method comprises: Performing preliminary processing on the glass substrate; Spray cleaning the glass substrate; Obtaining measurement data for glass substrate processing and determining a processing plan based on the measurement data; The glass substrate is processed according to the processing plan.

2. The photomask substrate processing method according to claim 1, characterized in that: The preliminary processing of the glass substrate includes: placing the glass substrate flat on the rubber vacuum suction cup of the engraving machine, and performing edge grinding, edge grinding, and chamfering processes.

3. The photomask substrate processing method according to claim 1, characterized in that: The spray cleaning of the glass substrate comprises: placing the glass substrate in a water tank, spray cleaning the front and back surfaces of the glass substrate, and after spray cleaning, using clean compressed air to blow dry water marks on the front and back surfaces of the glass substrate.

4. The photomask substrate processing method according to claim 3, characterized in that: The obtaining of the measurement data for glass substrate processing includes: using a flatness image tester to measure the flatness, parallelism, thickness and surface shape of the glass substrate, and calculating the total feed amount of the grinding process according to the surface shape of the glass substrate.

5. The photomask substrate processing method according to any one of claims 1 to 4, characterized in that: The processing scheme includes: The surface with poor flatness is selected as the front surface, and the other surface is selected as the back surface, and the front surface is the first surface to be processed; Grinding a glass substrate; The glass substrate is polished.

6. The photomask substrate processing method according to claim 5, characterized in that: The grinding process of the glass substrate comprises: placing the glass substrate flat on the magnetic work surface of the surface grinder, using precision gap gauges of different thicknesses to measure the adjacent gap between the raw material glass substrate and the work surface, filling and adjusting the gap by using precision gap gauges of appropriate thickness, selecting diamond grinding wheels of different particle sizes to sequentially perform rough grinding, semi-fine grinding, and fine grinding on the glass substrate, and spray cleaning the glass substrate after each grinding.

7. The photomask substrate processing method according to claim 6, characterized in that: The rough grinding method comprises: using a diamond grinding wheel with a particle size of 270# for rough grinding, the glass substrate reciprocates along the X-axis direction, the diamond grinding wheel continuously feeds along the Y-axis direction, after reciprocating once in the Y-axis direction, the diamond grinding wheel intermittently feeds once again along the Z-axis direction perpendicular to the front side of the glass substrate, after the front side of the glass substrate is roughly ground and spray-cleaned, the back side of the glass substrate is roughly ground and spray-cleaned, and the surface flatness of the glass substrate after grinding is measured.

8. The photomask substrate processing method according to claim 6, characterized in that: The semi-finishing grinding method comprises: using a diamond grinding wheel with a particle size of 500# for semi-finishing grinding, the glass substrate reciprocates along the X-axis direction, the diamond grinding wheel continuously feeds along the Y-axis direction, after reciprocating once in the Y-axis direction, the diamond grinding wheel intermittently feeds once again along the Z-axis direction perpendicular to the front side of the glass substrate, after semi-finishing grinding and spray cleaning of the front side of the glass substrate, semi-finishing grinding and spray cleaning of the back side of the glass substrate, and measuring the surface flatness of the glass substrate after grinding.

9. The photomask substrate processing method according to claim 6, characterized in that: The fine grinding method comprises: using a diamond grinding wheel with a particle size of 800#-1340# for fine grinding, the glass substrate reciprocates along the X-axis direction, the diamond grinding wheel continuously feeds along the Y-axis direction, after reciprocating once in the Y-axis direction, the diamond grinding wheel intermittently feeds once again along the Z-axis direction perpendicular to the front side of the glass substrate, after fine grinding and spray cleaning the front side of the glass substrate, fine grinding and spray cleaning the back side of the glass substrate, and measuring the surface flatness of the glass substrate after grinding.

10. The photomask substrate processing method according to claim 5, characterized in that: The polishing process of the glass substrate includes: sequentially performing rough polishing and fine polishing on the glass substrate; the rough polishing includes: after grinding, using a polishing device to perform chemical mechanical polishing on the raw material glass substrate, the glass substrate is placed flat in the star tray, the upper and lower surfaces thereof are in contact with the rough polishing pad, and polishing powder with a particle size of 1um-5um is selected; the fine polishing includes: after grinding, using a polishing device to perform chemical mechanical polishing on the raw material glass substrate, the glass substrate is placed flat in the star tray, the upper and lower surfaces thereof are in contact with the rough polishing pad, and polishing powder with a particle size of 0.5um-3um is selected.