Glass fiber prepreg and application thereof in fin structural member
Through the modification of modified calcium carbonate whiskers and nano-silica, the problem of poor dispersion of nano-silica in glass fiber prepreg is solved, forming a three-dimensional network structure, improving the strength and toughness of the composite material. It is suitable for on the flap structural part.
Patent Information
- Application Number
- CN202411095641.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
Nanosilicon dioxide is not easily dispersed evenly in glass fiber prepregs, resulting in weakening of toughening and strengthening effects, affecting the overall performance of the composite material.
Modified calcium carbonate whiskers and modified nanosilicon dioxide as toughening reinforcement agents, the roughness and group richness of its surface are improved by argon plasma and ultrasonic treatment, and a three-dimensional network structure is formed with epoxy resin. , enhance dispersion and binding force.
The strength, toughness and structural stability of the glass fiber prepreg composite material are significantly improved, ensuring its excellent application effect in flap structural parts.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of prepregs, and in particular relates to a glass fiber prepreg and application thereof in a wing structure. Background Art
[0002] Prepreg is a composite of reinforcing material and resin matrix made by impregnating continuous fibers or fabrics with resin matrix under strictly controlled conditions. It is an intermediate material for manufacturing fiber-reinforced resin-based composite materials. Prepreg uses lightweight fibers as the base material and combines it with high-performance resins, so that the material has excellent mechanical properties while maintaining a low density. Composite materials produced using prepreg can effectively improve the strength, corrosion resistance, fatigue life, wear resistance and impact resistance of the material, and can achieve lightweight composite materials. At present, prepreg has been widely used in the aerospace field.
[0003] In the field of aerospace technology, prepregs are needed to prepare aircraft wings, such as the tail fins of missiles. In the manufacturing process of missile tail fins, prepregs play an important role as a key material, which is crucial for reducing the weight of the wing and improving flight efficiency. In addition, the resin matrix in the prepreg usually has high heat resistance and can maintain stable performance in high temperature environments, ensuring the safety and reliability of the wing under extreme working conditions.
[0004] Since the wing is crucial to the flight stability and attitude control of the aircraft, it is necessary to use prepregs with excellent performance to manufacture the wing to ensure the safety and reliability of the aircraft. Among them, glass fiber prepreg is one of the commonly used materials.
[0005] In order to further enhance the strength and toughness of glass fiber reinforced resin-based composite materials prepared from glass fiber prepreg, nano-silicon dioxide is often used for toughening and strengthening. Although the addition of nano-silicon dioxide can bring many advantages, nano-silicon dioxide is not easy to be evenly dispersed in the resin matrix due to its high specific surface area and surface energy, and agglomeration is easy to occur in the resin matrix. In addition, the interfacial bonding force between nano-silicon dioxide and the resin matrix is not strong enough. The above defects will weaken the toughening and strengthening effect of nano-silicon dioxide, and may also affect the overall performance of the prepreg. Summary of the invention
[0006] The present invention provides a glass fiber prepreg and application thereof in a wing structure. The composite material prepared by using the glass fiber prepreg of the present invention has high strength, good toughness, strong structural stability, and has a good application effect in the wing structure.
[0007] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0008] A glass fiber prepreg, the glass fiber prepreg comprising the following raw materials in weight percentage: 55-60% glass fiber cloth, 40-45% epoxy resin mixture;
[0009] The epoxy resin mixture comprises the following raw materials in parts by weight: 100 parts of epoxy resin, 2.5-3.8 parts of toughening and reinforcing agent, 28-35 parts of curing agent, and 1-2 parts of curing accelerator; the toughening and reinforcing agent is composed of modified calcium carbonate whisker and modified nano silicon dioxide in a mass ratio of 1:0.5-1.
[0010] Preferably, the preparation method of the modified calcium carbonate whisker comprises the following steps:
[0011] First, the calcium carbonate whiskers are subjected to argon plasma treatment, the argon plasma treatment time is 60-90s, and the power is 200-400W, to obtain argon plasma modified calcium carbonate whiskers;
[0012] Dopamine hydrochloride is added to a Tris-HCl buffer solution with a pH value of 8.5-9, and after stirring and mixing, argon plasma is added to modify calcium carbonate whiskers, and then ultrasonic treatment is performed for 3-6 hours while stirring, and then centrifugation, water washing, and drying are performed in sequence to obtain modified calcium carbonate whiskers; the mass volume ratio of the calcium carbonate whiskers, dopamine hydrochloride, and Tris-HCl buffer solution is 1g: 0.3-0.6g: 500-1000ml.
[0013] Preferably, the diameter of the calcium carbonate whisker is 1-3 μm and the length is 30-60 μm; the concentration of the Tris-HCl buffer solution is 0.05-0.1 mol / L; in the stirring and ultrasonic treatment, the stirring speed is 100-200 r / min, and the power of the ultrasonic treatment is 200-500W.
[0014] Preferably, the preparation method of the modified nano-silicon dioxide comprises the following steps:
[0015] First, the nano-silicon dioxide is treated with argon plasma, the argon plasma treatment time is 30-60s, the power is 200-400W, and the argon plasma modified nano-silicon dioxide is obtained;
[0016] Dopamine hydrochloride is added to a Tris-HCl buffer solution with a pH value of 8.5-9, and after stirring and mixing, nano-silicon dioxide is added, and then ultrasonic treatment is performed for 2.5-5 hours while stirring, and then centrifugation, water washing, and drying are performed in sequence to obtain modified nano-silicon dioxide; the mass volume ratio of the nano-silicon dioxide, dopamine hydrochloride, and Tris-HCl buffer solution is 1g: 0.2-0.5g: 500-1000ml.
[0017] Preferably, the particle size of the nano-silicon dioxide is 50-100 nm; the concentration of the Tris-HCl buffer solution is 0.05-0.1 mol / L; during the ultrasonic treatment with stirring, the stirring speed is 300-400 r / min, and the power of the ultrasonic treatment is 200-500W.
[0018] Preferably, the glass fiber cloth is a modified glass fiber unidirectional cloth, and the preparation method of the modified glass fiber unidirectional cloth comprises the following steps:
[0019] First, the glass fiber unidirectional cloth is subjected to argon plasma treatment, the argon plasma treatment time is 5-10 minutes, the power is 200-500W, and the argon plasma modified glass fiber unidirectional cloth is obtained;
[0020] The argon plasma modified glass fiber unidirectional cloth is treated with oxygen plasma. The oxygen plasma treatment time is 2-3 minutes and the power is 500-800W to obtain the modified glass fiber unidirectional cloth.
[0021] Preferably, the epoxy resin is bisphenol A type liquid epoxy resin.
[0022] Preferably, the curing agent is one or more of D230 and D400, and the curing accelerator is DMP-30.
[0023] Preferably, the method for preparing the glass fiber prepreg comprises the following steps:
[0024] S1: Add a toughening and reinforcing agent to the epoxy resin, heat it to 60-65°C, stir and mix, then add a curing agent and a curing accelerator, stir and mix, to obtain an epoxy resin mixture;
[0025] S2: Evenly coat the epoxy resin mixture on the release paper at a coating temperature of 60-65°C to prepare an upper resin film and a lower resin film with release paper; attach the upper resin film and the lower resin film with release paper to the upper and lower sides of the glass fiber cloth respectively, and heat-press and laminate them with a roller at a lamination temperature of 65-70°C, and then cool them to prepare the glass fiber prepreg.
[0026] As a general inventive concept, the present invention provides an application of the above-mentioned glass fiber prepreg in a wing structure, wherein the wing structure includes an aluminum alloy frame and a composite material skin, and the cavity between the aluminum alloy frame and the composite material skin is filled with foam; the foam is polymethacrylimide foam, and the composite material skin is prepared from the glass fiber prepreg.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. The toughening and reinforcing agent in the glass fiber prepreg of the present invention is composed of modified calcium carbonate whisker and modified nano silicon dioxide, wherein the modified calcium carbonate whisker and modified nano silicon dioxide are calcium carbonate whisker, silicon dioxide are successively modified by argon plasma and polydopamine, by the above-mentioned modification, the roughness of the surface of calcium carbonate whisker and nano silicon dioxide is increased, and the groups on its surface are rich, not only the dispersion performance is effectively improved, but also the bonding force between the epoxy resin matrix is high and tightly combined. And the present invention adopts modified calcium carbonate whisker and modified nano silicon dioxide to coordinate, wherein the modified calcium carbonate whisker can form a three-dimensional network structure in the matrix after being dispersed in the epoxy resin matrix, thereby the agglomeration of nano silicon dioxide can be further suppressed, and then the high dispersibility of nano silicon dioxide is better maintained, so that it gives full play to the reinforcing performance, and the calcium carbonate crystal itself can also effectively enhance the strength, toughness, etc. of the material, so that the structural strength and structural stability of the composite material prepared by the glass fiber prepreg of the present invention are further enhanced.
[0029] 2. When the calcium carbonate whisker and nano-silicon dioxide are modified by the present invention, argon plasma modification is first performed, and then polydopamine modification is performed, and the amount of dopamine hydrochloride used is controlled within a small range, thereby reducing the amount of polydopamine grafted to the calcium carbonate whisker and nano-silicon dioxide. Through the above operation, not only the dispersibility of the calcium carbonate whisker and nano-silicon dioxide is improved, but also the calcium carbonate whisker and nano-silicon dioxide have a strong bonding force with the epoxy resin matrix, and the problems of poor interface bonding performance and enhanced water absorption of materials caused by excessive polydopamine are avoided. Poor interface bonding performance and enhanced water absorption of materials may have a certain impact on the structural stability of the composite material prepared by the glass fiber prepreg, while the wing structure has high requirements for the structural stability of the composite material.
[0030] 3. In addition to using a specific toughening and reinforcing agent, the present invention also sequentially performs argon plasma modification and oxygen plasma modification on the glass fiber unidirectional cloth, which not only significantly increases the surface roughness of the glass fiber unidirectional cloth, but also enriches the active groups on the surface, thereby significantly enhancing the bonding force between the obtained glass fiber cloth and the epoxy resin matrix, thereby effectively improving the mechanical properties of the composite material prepared from the glass fiber prepreg of the present invention.
[0031] 4. The composite material prepared from the glass fiber prepreg of the present invention has high strength, good toughness, strong structural stability, and has a good application effect in wing structural parts. DETAILED DESCRIPTION
[0032] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the preferred embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.
[0033] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0035] Preparation Example 1:
[0036] A method for preparing a modified glass fiber unidirectional cloth comprises the following steps:
[0037] First, the glass fiber unidirectional cloth (surface density 110±1g / m 2 ) performing argon plasma treatment, the argon plasma treatment time is 10 min, the power is 200 W, and an argon plasma modified glass fiber unidirectional cloth is obtained;
[0038] The argon plasma modified glass fiber unidirectional cloth was treated with oxygen plasma. The oxygen plasma treatment time was 2 minutes and the power was 800 W to obtain a modified glass fiber unidirectional cloth.
[0039] Preparation Example 2:
[0040] A method for preparing a modified glass fiber unidirectional cloth comprises the following steps:
[0041] First, the glass fiber unidirectional cloth (surface density 110±1g / m 2 ) performing argon plasma treatment, the argon plasma treatment time is 5 min, the power is 500 W, and an argon plasma modified glass fiber unidirectional cloth is obtained;
[0042] The argon plasma modified glass fiber unidirectional cloth was treated with oxygen plasma. The oxygen plasma treatment time was 3 minutes and the power was 500 W to obtain a modified glass fiber unidirectional cloth.
[0043] Preparation Example 3:
[0044] A method for preparing modified calcium carbonate whiskers comprises the following steps:
[0045] First, calcium carbonate whiskers with a diameter of 1-3 μm and a length of 30-60 μm are treated with argon plasma. The argon plasma treatment time is 80 seconds and the power is 400 W to obtain argon plasma modified calcium carbonate whiskers;
[0046] Dopamine hydrochloride is added to a Tris-HCl buffer solution with a pH value of 8.5, and after stirring and mixing, argon plasma modified calcium carbonate whiskers are added, and then ultrasonic treatment is performed for 6 hours while stirring, the stirring speed is 100 r / min, and the power of the ultrasonic treatment is 200 W; then centrifugation, water washing, and drying are performed in sequence to obtain modified calcium carbonate whiskers;
[0047] The mass volume ratio of the calcium carbonate whisker, dopamine hydrochloride and Tris-HCl buffer solution is 1g:0.3g:500ml; the concentration of the Tris-HCl buffer solution is 0.06mol / L.
[0048] Preparation Example 4:
[0049] A method for preparing modified calcium carbonate whiskers comprises the following steps:
[0050] First, calcium carbonate whiskers with a diameter of 1-3 μm and a length of 30-60 μm are treated with argon plasma. The argon plasma treatment time is 60 seconds and the power is 200 W to obtain argon plasma modified calcium carbonate whiskers;
[0051] Dopamine hydrochloride is added to a Tris-HCl buffer solution with a pH value of 8.5, and after stirring and mixing, argon plasma is added to modify calcium carbonate whiskers, and then ultrasonic treatment is performed for 3 hours while stirring, the stirring speed is 200 r / min, and the power of the ultrasonic treatment is 300 W; then centrifugation, water washing, and drying are performed in sequence to obtain modified calcium carbonate whiskers;
[0052] The mass volume ratio of the calcium carbonate whisker, dopamine hydrochloride and Tris-HCl buffer solution is 1 g:0.6 g:1000 ml; the concentration of the Tris-HCl buffer solution is 0.05 mol / L.
[0053] Preparation Example 5:
[0054] A method for preparing modified calcium carbonate whiskers comprises the following steps:
[0055] First, calcium carbonate whiskers with a diameter of 1-3 μm and a length of 30-60 μm are treated with argon plasma. The argon plasma treatment time is 90 seconds and the power is 200 W to obtain argon plasma modified calcium carbonate whiskers;
[0056] Dopamine hydrochloride is added to a Tris-HCl buffer solution with a pH value of 9, and after stirring and mixing, argon plasma is added to modify calcium carbonate whiskers, and then ultrasonic treatment is performed for 5 hours while stirring, the stirring speed is 200 r / min, and the power of the ultrasonic treatment is 500 W; then centrifugation, water washing, and drying are performed in sequence to obtain modified calcium carbonate whiskers;
[0057] The mass volume ratio of the calcium carbonate whisker, dopamine hydrochloride and Tris-HCl buffer solution is 1g:0.5g:800ml; the concentration of the Tris-HCl buffer solution is 0.1mol / L.
[0058] Preparation Example 6:
[0059] A method for preparing modified nano-silicon dioxide comprises the following steps:
[0060] First, nano-silicon dioxide with a particle size of 50-100 nm is treated with argon plasma. The argon plasma treatment time is 60 seconds and the power is 200W to obtain argon plasma modified nano-silicon dioxide;
[0061] Dopamine hydrochloride is added to a Tris-HCl buffer solution with a pH value of 8.5, and after stirring and mixing, nano-silicon dioxide is added, and then ultrasonic treatment is performed for 3 hours while stirring, the stirring speed is 400r / min, and the power of the ultrasonic treatment is 300W; then centrifugation, water washing, and drying are performed in sequence to obtain modified nano-silicon dioxide;
[0062] The mass volume ratio of the nano-silicon dioxide, dopamine hydrochloride and Tris-HCl buffer solution is 1g:0.2g:500ml; the concentration of the Tris-HCl buffer solution is 0.05mol / L.
[0063] Preparation Example 7:
[0064] A method for preparing modified nano-silicon dioxide comprises the following steps:
[0065] First, nano-silicon dioxide with a particle size of 50-100 nm is treated with argon plasma. The argon plasma treatment time is 50 seconds and the power is 200W to obtain argon plasma modified nano-silicon dioxide;
[0066] Dopamine hydrochloride is added to a Tris-HCl buffer solution with a pH value of 9, and after stirring and mixing, nano-silicon dioxide is added, and then ultrasonic treatment is performed for 5 hours while stirring, the stirring speed is 300r / min, and the power of the ultrasonic treatment is 200W; then centrifugation, water washing, and drying are performed in sequence to obtain modified nano-silicon dioxide;
[0067] The mass volume ratio of the nano-silicon dioxide, dopamine hydrochloride and Tris-HCl buffer solution is 1g:0.5g:1000ml; the concentration of the Tris-HCl buffer solution is 0.1mol / L.
[0068] Preparation Example 8:
[0069] A method for preparing modified nano-silicon dioxide comprises the following steps:
[0070] First, nano-silicon dioxide with a particle size of 50-100 nm is treated with argon plasma. The argon plasma treatment time is 30 seconds and the power is 200W to obtain argon plasma modified nano-silicon dioxide;
[0071] Dopamine hydrochloride is added to a Tris-HCl buffer solution with a pH value of 9, and after stirring and mixing, nano-silicon dioxide is added, and then ultrasonic treatment is performed for 2.5 hours while stirring, the stirring speed is 400r / min, and the power of the ultrasonic treatment is 500W; then centrifugation, water washing, and drying are performed in sequence to obtain modified nano-silicon dioxide;
[0072] The mass volume ratio of the nano-silicon dioxide, dopamine hydrochloride and Tris-HCl buffer solution is 1g:0.4g:1000ml; the concentration of the Tris-HCl buffer solution is 0.1mol / L.
[0073] Embodiment 1:
[0074] A glass fiber prepreg comprises the following raw materials in percentage by weight: 55% of modified glass fiber unidirectional cloth and 45% of epoxy resin mixture;
[0075] The epoxy resin mixture includes the following raw materials in parts by weight: 100 parts of epoxy resin NPEL-127, 3.2 parts of toughening and reinforcing agent, 30 parts of curing agent D230, and 1 part of curing accelerator DMP-30; the toughening and reinforcing agent is composed of modified calcium carbonate whiskers and modified nano silicon dioxide in a mass ratio of 1:0.7.
[0076] The modified glass fiber unidirectional cloth is prepared by the method in Preparation Example 1; the modified calcium carbonate whisker is prepared by the method in Preparation Example 4; and the modified nano-silicon dioxide is prepared by the method in Preparation Example 6.
[0077] The preparation method of glass fiber prepreg comprises the following steps:
[0078] S1: Add toughening and reinforcing agent to epoxy resin NPEL-127, heat to 60°C and stir to mix, then add curing agent D230 and curing accelerator DMP-30 and stir to mix to obtain epoxy resin mixture;
[0079] S2: The epoxy resin mixture is evenly coated on the release paper at a coating temperature of 60°C to prepare an upper resin film and a lower resin film with release paper; the upper resin film and the lower resin film with release paper are respectively attached to the upper and lower sides of the modified glass fiber unidirectional cloth, and are hot-pressed and laminated by rollers at a lamination temperature of 68°C, and then cooled to prepare a glass fiber prepreg.
[0080] Embodiment 2:
[0081] A glass fiber prepreg comprises the following raw materials in percentage by weight: 57% of modified glass fiber unidirectional cloth and 43% of epoxy resin mixture;
[0082] The epoxy resin mixture includes the following raw materials in parts by weight: 100 parts of epoxy resin NPEL-127, 2.5 parts of toughening and reinforcing agent, 30 parts of curing agent D230, and 1.5 parts of curing accelerator DMP-30; the toughening and reinforcing agent is composed of modified calcium carbonate whisker and modified nano silicon dioxide in a mass ratio of 1:0.5.
[0083] The modified glass fiber unidirectional cloth is prepared by the method in Preparation Example 2; the modified calcium carbonate whisker is prepared by the method in Preparation Example 3; and the modified nano-silicon dioxide is prepared by the method in Preparation Example 8.
[0084] The preparation method of glass fiber prepreg comprises the following steps:
[0085] S1: Add toughening and reinforcing agent to epoxy resin NPEL-127, heat to 65°C, stir and mix, then add curing agent D230 and curing accelerator DMP-30, stir and mix to obtain epoxy resin mixture;
[0086] S2: The epoxy resin mixture is evenly coated on the release paper at a coating temperature of 65°C to prepare an upper resin film and a lower resin film with release paper; the upper resin film and the lower resin film with release paper are respectively attached to the upper and lower sides of the modified glass fiber unidirectional cloth, and are hot-pressed and laminated by rollers at a lamination temperature of 70°C, and then cooled to prepare a glass fiber prepreg.
[0087] Embodiment 3:
[0088] A glass fiber prepreg comprises the following raw materials in percentage by weight: 60% of modified glass fiber unidirectional cloth and 40% of epoxy resin mixture;
[0089] The epoxy resin mixture includes the following raw materials in parts by weight: 100 parts of epoxy resin NPEL-127, 3 parts of toughening and reinforcing agent, 28 parts of curing agent D230, and 2 parts of curing accelerator DMP-30; the toughening and reinforcing agent is composed of modified calcium carbonate whisker and modified nano silicon dioxide in a mass ratio of 1:1.
[0090] The modified glass fiber unidirectional cloth is prepared by the method in Preparation Example 1; the modified calcium carbonate whisker is prepared by the method in Preparation Example 3; and the modified nano-silicon dioxide is prepared by the method in Preparation Example 8.
[0091] The preparation method of glass fiber prepreg comprises the following steps:
[0092] S1: Add toughening and reinforcing agent to epoxy resin NPEL-127, heat to 62°C, stir and mix, then add curing agent D230 and curing accelerator DMP-30, stir and mix to obtain epoxy resin mixture;
[0093] S2: The epoxy resin mixture is evenly coated on the release paper at a coating temperature of 64°C to prepare an upper resin film and a lower resin film with release paper; the upper resin film and the lower resin film with release paper are respectively attached to the upper and lower sides of the modified glass fiber unidirectional cloth, and are hot-pressed and laminated by rollers at a lamination temperature of 65°C, and then cooled to prepare a glass fiber prepreg.
[0094] Embodiment 4:
[0095] A glass fiber prepreg comprises the following raw materials in percentage by weight: 58% of modified glass fiber unidirectional cloth and 42% of epoxy resin mixture;
[0096] The epoxy resin mixture includes the following raw materials in parts by weight: 100 parts of epoxy resin NPEL-127, 3.8 parts of toughening and reinforcing agent, 35 parts of curing agent D230, and 1.5 parts of curing accelerator DMP-30; the toughening and reinforcing agent is composed of modified calcium carbonate whisker and modified nano silicon dioxide in a mass ratio of 1:0.5.
[0097] The modified glass fiber unidirectional cloth is prepared by the method in Preparation Example 2; the modified calcium carbonate whisker is prepared by the method in Preparation Example 5; and the modified nano-silicon dioxide is prepared by the method in Preparation Example 6.
[0098] The preparation method of the glass fiber prepreg is the same as that of Example 1.
[0099] Embodiment 5:
[0100] A glass fiber prepreg comprises the following raw materials in percentage by weight: 56% of modified glass fiber unidirectional cloth and 44% of epoxy resin mixture;
[0101] The epoxy resin mixture includes the following raw materials in parts by weight: 100 parts of epoxy resin NPEL-127, 2.8 parts of toughening and reinforcing agent, 32 parts of curing agent D230, and 1.5 parts of curing accelerator DMP-30; the toughening and reinforcing agent is composed of modified calcium carbonate whisker and modified nano silicon dioxide in a mass ratio of 1:0.8.
[0102] The modified glass fiber unidirectional cloth is prepared by the method in Preparation Example 2; the modified calcium carbonate whisker is prepared by the method in Preparation Example 5; and the modified nano-silicon dioxide is prepared by the method in Preparation Example 7.
[0103] The preparation method of the glass fiber prepreg is the same as that of Example 2.
[0104] Embodiment 6:
[0105] A wing structure comprises an aluminum alloy frame and a composite material skin, wherein the cavity between the aluminum alloy frame and the composite material skin is filled with foam; the foam is polymethacrylimide foam, and the composite material skin is prepared from the glass fiber prepreg in Examples 1-5.
[0106] Comparative Example 1:
[0107] A glass fiber prepreg, which is different from Example 1 in that the toughening and reinforcing agent is modified nano-silicon dioxide.
[0108] Comparative Example 2:
[0109] A glass fiber prepreg, which is different from Example 1 in that the toughening and reinforcing agent is modified calcium carbonate whisker.
[0110] Comparative Example 3:
[0111] A glass fiber prepreg, different from Example 1, the toughening and reinforcing agent is composed of calcium carbonate whiskers and nano silicon dioxide in a mass ratio of 1:0.8. The diameter of the calcium carbonate whiskers is 1-3 μm and the length is 30-60 μm, and the particle size of the nano silicon dioxide is 50-100 nm.
[0112] Performance Testing:
[0113] According to the glass fiber prepreg in Examples 1-5 and Comparative Examples 1-2, glass fiber reinforced resin composite material samples were prepared after curing and molding, and the curing system during curing and molding was 100°C / 1.5h+130°C / 2h. The prepared glass fiber reinforced resin composite material samples were tested for 0° tensile strength, 0° tensile modulus, and 0° bending strength. The test methods for 0° tensile strength and 0° tensile modulus adopted "GB / T 1447-2005 Test Method for Tensile Properties of Fiber Reinforced Plastics"; the test method for 0° bending strength adopted "GB / T 1449-2005 Test Method for Bending Properties of Fiber Reinforced Plastics", and the specific mechanical test results are shown in Table 1.
[0114] Table 1 Mechanical properties test results
[0115]
[0116]
[0117] As shown in Table 1, the glass fiber reinforced resin composite material prepared by the glass fiber prepreg obtained by the method in Examples 1-5 of the present invention has excellent mechanical properties, high strength and good toughness, and has a good application effect in the wing structure, which is beneficial to improve the overall mechanical performance of the wing structure and reduce the production cost. However, as shown in Comparative Examples 1-3 and Example 6, if modified calcium carbonate whiskers or modified nano-silicon dioxide are used alone as toughening and reinforcing agents, or unmodified calcium carbonate whiskers and nano-silicon dioxide are used as toughening and reinforcing agents, the mechanical properties of the glass fiber reinforced resin composite material prepared by the glass fiber prepreg are significantly reduced.
[0118] The above are preferred embodiments of the present invention, but the present invention is not limited to the described embodiments. It should be noted that for those skilled in the art, without departing from the principles of the present invention, changes, improvements and modifications to these embodiments should be considered as the protection scope of the present invention.
Claims
1. A glass fiber prepreg, characterized in that: The glass fiber prepreg comprises the following raw materials in weight percentage: 55-60% glass fiber cloth and 40-45% epoxy resin mixture; The epoxy resin mixture comprises the following raw materials in parts by weight: 100 parts of epoxy resin, 2.5-3.8 parts of toughening and reinforcing agent, 28-35 parts of curing agent, and 1-2 parts of curing accelerator; the toughening and reinforcing agent is composed of modified calcium carbonate whisker and modified nano silicon dioxide in a mass ratio of 1:0.5-1.
2. The glass fiber prepreg according to claim 1, characterized in that The preparation method of the modified calcium carbonate whisker comprises the following steps: First, the calcium carbonate whiskers are subjected to argon plasma treatment, the argon plasma treatment time is 60-90s, and the power is 200-400W, to obtain argon plasma modified calcium carbonate whiskers; Dopamine hydrochloride is added to a Tris-HCl buffer solution with a pH value of 8.5-9, and after stirring and mixing, argon plasma is added to modify calcium carbonate whiskers, and then ultrasonic treatment is performed for 3-6 hours while stirring, and then centrifugation, water washing, and drying are performed in sequence to obtain modified calcium carbonate whiskers; the mass volume ratio of the calcium carbonate whiskers, dopamine hydrochloride, and Tris-HCl buffer solution is 1g: 0.3-0.6g: 500-1000ml.
3. The glass fiber prepreg according to claim 2, characterized in that: The diameter of the calcium carbonate whisker is 1-3 μm, and the length is 30-60 μm; the concentration of the Tris-HCl buffer solution is 0.05-0.1 mol / L; in the stirring and ultrasonic treatment, the stirring speed is 100-200 r / min, and the power of the ultrasonic treatment is 200-500W.
4. The glass fiber prepreg according to claim 1, characterized in that: The preparation method of the modified nano silicon dioxide comprises the following steps: First, the nano-silicon dioxide is treated with argon plasma, the argon plasma treatment time is 30-60s, the power is 200-400W, and the argon plasma modified nano-silicon dioxide is obtained; Dopamine hydrochloride is added to a Tris-HCl buffer solution with a pH value of 8.5-9, and after stirring and mixing, nano-silicon dioxide is added, and then ultrasonic treatment is performed for 2.5-5 hours while stirring, and then centrifugation, water washing, and drying are performed in sequence to obtain modified nano-silicon dioxide; the mass volume ratio of the nano-silicon dioxide, dopamine hydrochloride, and Tris-HCl buffer solution is 1g: 0.2-0.5g: 500-1000ml.
5. The glass fiber prepreg according to claim 4, characterized in that: The particle size of the nano-silicon dioxide is 50-100nm; the concentration of the Tris-HCl buffer solution is 0.05-0.1mol / L; during the stirring and ultrasonic treatment, the stirring speed is 300-400r / min, and the power of the ultrasonic treatment is 200-500W.
6. The glass fiber prepreg according to claim 1, characterized in that: The glass fiber cloth is a modified glass fiber unidirectional cloth, and the preparation method of the modified glass fiber unidirectional cloth comprises the following steps: First, the glass fiber unidirectional cloth is subjected to argon plasma treatment, the argon plasma treatment time is 5-10 minutes, the power is 200-500W, and the argon plasma modified glass fiber unidirectional cloth is obtained; The argon plasma modified glass fiber unidirectional cloth is treated with oxygen plasma. The oxygen plasma treatment time is 2-3 minutes and the power is 500-800W to obtain the modified glass fiber unidirectional cloth.
7. The glass fiber prepreg according to claim 1, characterized in that: The epoxy resin is bisphenol A type liquid epoxy resin.
8. The glass fiber prepreg according to claim 1, characterized in that: The curing agent is one or more of D230 and D400, and the curing accelerator is DMP-30.
9. The glass fiber prepreg according to claim 1, characterized in that: The preparation method of the glass fiber prepreg comprises the following steps: S1: Add a toughening and reinforcing agent to the epoxy resin, heat it to 60-65°C, stir and mix, then add a curing agent and a curing accelerator, stir and mix, to obtain an epoxy resin mixture; S2: The epoxy resin mixture is evenly coated on the release paper at a coating temperature of 60-65°C to prepare an upper resin film and a lower resin film with release paper; the upper resin film and the lower resin film with release paper are respectively attached to the upper and lower sides of the glass fiber cloth, and are hot-pressed and laminated by rollers at a lamination temperature of 65-70°C, and then cooled to prepare a glass fiber prepreg.
10. An application of the glass fiber prepreg as described in any one of claims 1 to 9 in a wing structure, the wing structure comprising an aluminum alloy skeleton and a composite material skin, the cavity between the aluminum alloy skeleton and the composite material skin is filled with foam; the foam is polymethacrylimide foam, and the composite material skin is prepared from the glass fiber prepreg.
Citation Information
Cited By
Preparation method of carbonized polydopamine / spent bleaching clay reinforced self-lubricating fabric composite material
CN119711156A
Preparation method of carbonized polydopamine / waste clay reinforced self-lubricating fabric composite material
CN119711156B