Light carbonization anti-deformation multilayer board and manufacturing method thereof
By combining light carbonization treatment technology and glue layer materials, the deformation problem of multi-layer boards when using poplar isotope is solved, which significantly improves the deformation resistance and stability, realizes energy saving and emission reduction and green production, and is suitable for furniture. Manufacturing and other industries.
Patent Information
- Application Number
- CN202411356231.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-22
AI Technical Summary
The existing multi-layer boards are prone to deform due to poor stability when using poplar isometric raw materials, resulting in insufficient anti-deformation performance, which limits its wide application in the furniture industry.
Light carbonization full carbon treatment, light carbonization interval carbon treatment, light carbonization surface carbon treatment, light carbonization paraffin coating and light carbonization steam spraying technology are adopted, and light carbonization anti-deformation multi-layer structure is formed with different carbonization temperatures and times. The board is made of rubber layer materials such as urea formaldehyde resin and phenolic resin to optimize the stability and deformation resistance of the board.
It significantly improves the anti-deformation performance and stability of multi-layer boards, reduces energy consumption and production costs, realizes green and low-carbon production, enhances the dimensional stability and mechanical properties of the boards, and is suitable for different environmental conditions.
Smart Images

Figure CN118991183A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of physical mechanics of furniture boards, and in particular to a light carbonized anti-deformation multilayer board and a manufacturing method thereof. Background Art
[0002] Multilayer boards occupy a core position in the vast field of man-made boards, especially in the three major mainstream boards - multilayer boards, particle boards, and fiberboards, where their production and sales volume is the best. After decades of rapid development, multilayer boards have become the dominant force in my country's man-made board industry. In February 2024, the latest statistics released by the Industrial Development Planning Institute of the State Forestry and Grassland Administration and the China Forest Products Industry Association showed that there are 1,477 multilayer board production companies under construction in China, with an annual design production capacity of approximately 28.9 million cubic meters. This data strongly proves that multilayer boards have a strong position at the top of the list in my country's man-made board market.
[0003] However, the furniture manufacturing industry has extremely high requirements for the quality and performance of the board materials, which is directly related to the quality and service life of the furniture. The deformation problem of multi-layer boards, especially when using fast-growing materials such as poplar, has become the main obstacle to the wider application of multi-layer boards in the furniture industry due to their poor stability and easy deformation. Therefore, the research and development of multi-layer boards with excellent anti-deformation properties can not only significantly improve the quality of furniture and extend its service life, but also is the key to promoting the high-quality development of the furniture manufacturing industry. For the entire industry, this is not only a hot spot for innovative research, but also has far-reaching practical significance.
[0004] After in-depth literature search and technical comparison, it was found that a related patent (publication number CN103692505B) revealed a carbonized plywood and its production method, which uses a continuous hot press to carbonize the veneer, followed by gluing and cold pressing, with cold-curing adhesive as the key raw material. However, this technology still has room for improvement in terms of energy-saving effects, depth and uniformity of carbonization treatment. The problem of failing to effectively release internal stress directly restricts the further optimization of the stability and anti-deformation properties of the board. This means that although the current technology has achieved certain results, on the road to achieving higher efficiency and better quality, more advanced processing methods and process improvements still need to be explored.
[0005] In order to break through this technical bottleneck, after long-term experiments and research, the present invention creatively integrates five major technologies: light carbonization full carbonization treatment, light carbonization interval carbonization treatment, light carbonization surface carbonization treatment, light carbonization paraffin coating and light carbonization steam spraying, and develops a set of optimal carbonization treatment solutions specifically for the characteristics and materials of fast-growing wood. The integrated application of this series of innovative technologies not only greatly improves the anti-deformation performance and overall quality of multi-layer boards, but also achieves the green production goal of energy conservation and emission reduction, showing great application potential in the production of anti-deformation artificial boards.
[0006] Compared with the existing technology, the present invention effectively eliminates the internal stress of the board through refined carbonization treatment and optimization of fast-growing materials, greatly improves the stability and anti-deformation ability of the board, and creates a new technical path in the field of anti-deformation artificial boards, which has innovative application value. Summary of the invention
[0007] In order to overcome the shortcomings of existing artificial boards that are easy to deform due to moisture absorption and have weak controllability, the present invention provides a light carbonized anti-deformation multilayer board and a manufacturing method thereof.
[0008] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0009] The invention discloses a light carbonization anti-deformation multilayer board, comprising a light carbonization layer and a glue layer, characterized in that the base material of the light carbonization layer is sprayed with high-temperature steam before carbonization or coated with a waterproofing agent after carbonization, or is a combination of the two or no treatment; the light carbonization anti-deformation multilayer board is assembled in a full carbonization manner; or in an interval carbonization manner; or in a surface carbonization manner; the light carbonization anti-deformation multilayer board is a board in which all multi-layer light carbonization structures are assembled into 3 layers, 5 layers, 7 layers, or an odd number of layers; the interval carbon is a symmetrical assembly of multi-layer light carbonization structures; the surface carbon is a board in which at least two layers of light carbonization structures respectively constitute the upper and lower surfaces of the multilayer board; the carbonization temperature of the light carbonization layer is 190-220°C, and the carbonization time is 3-15min; the glue layer includes but is not limited to urea-formaldehyde resin, phenolic resin and melamine glue or hydrophobic adhesive, thereby improving the anti-deformation performance of the board. Compared with traditional carbonization, light carbonization treatment shows excellent energy-saving characteristics, and significantly reduces energy consumption compared to the high-temperature and long-time treatment required by traditional carbonization. It reduces production costs and meets the current society's pursuit of green and low-carbon production methods. The experimental results clearly show that the light carbonization anti-deformation multilayer board surpasses other structural boards of the same thickness in anti-deformation performance, and its dimensional stability has been significantly enhanced.
[0010] The light carbonization anti-deformation multilayer board and the manufacturing method thereof are characterized in that: the light carbonization anti-deformation multilayer board and the manufacturing method thereof include a full carbon type blanking process production mode, an interval carbon type blanking process production mode, a surface carbon blanking process production mode, a paraffin coating process production mode, and a steam spraying process production mode, and include the following steps:
[0011] The light carbonization full carbon assembly process production method includes
[0012] S1: Peel the fast-growing poplar or other fast-growing wood into 2440×1220mm veneers with a veneer thickness of 1-3mm and a veneer thickness of 1-3mm;
[0013] S2: Place the poplar veneer described in S1 in a continuous veneer carbonization line or veneer carbonization kiln, set the temperature to 200°C, and lightly carbonize for 3-15 minutes, while introducing inert gas or carbon dioxide gas during light carbonization.
[0014] The light carbonized layer (1) can be obtained;
[0015] S3: brushing the lightly carbonized layers (1) treated in S2 with adhesive layers (2) respectively, and the gluing method is orthogonal gluing and then pressurizing, and curing, and finally forming a lightly carbonized full-carbon anti-deformation multilayer board with an odd number of layers;
[0016] The light carbonization interval assembly process production method includes
[0017] S1: Peel the fast-growing poplar or other fast-growing materials into 2440×1220mm veneers with a thickness of 1-3mm;
[0018] S2: placing the poplar veneer described in S1 in a continuous veneer carbonization line or a veneer carbonization kiln, setting the temperature to 200° C., lightly carbonizing for 3-15 minutes, and introducing inert gas or carbon dioxide gas during the light carbonization to obtain the lightly carbonized layer (1);
[0019] S3: brushing the lightly carbonized layer (1) treated in S2 with a glue layer (2) respectively, and assembling the blanks in an interval-type symmetrical manner, wherein the first layer is the lightly carbonized layer (1), the second layer is not carbonized, the third layer is the lightly carbonized layer (1), and so on to form an interval-type symmetrical blank assembly structure;
[0020] S4: orthogonally gluing the symmetrical blank structure completed in S3 and then applying pressure to solidify it, and finally forming a light carbonized interval anti-deformation multilayer board with an odd number of layers;
[0021] Light carbonization surface carbon assembly process production methods include
[0022] S1: Peel the fast-growing poplar or other fast-growing materials into 2440×1220mm veneers with a thickness of 1-3mm;
[0023] S2: placing the poplar veneer described in S1 in a continuous veneer carbonization line or a veneer carbonization kiln, setting the temperature to 200° C., lightly carbonizing for 3-15 minutes, and introducing inert gas or carbon dioxide gas during the light carbonization to obtain the lightly carbonized layer (1);
[0024] S3: brushing the lightly carbonized layer (1) treated in S2 with a glue layer (2) respectively, and assembling the blanks symmetrically according to the upper and lower surface layers, wherein the upper and lower surface layers are the lightly carbonized layer (1), and the remaining middle layers are all uncarbonized structures;
[0025] S4: orthogonally gluing the surface symmetrical assembly structure completed in S3 and then applying pressure and curing, and finally forming a lightly carbonized surface carbon anti-deformation multilayer board with an odd number of layers;
[0026] Light carbonized paraffin coating process production methods include
[0027] S1: Peel the fast-growing poplar or other fast-growing materials into 2440×1220mm veneers with a thickness of 1-3mm;
[0028] S2: Place the poplar veneer described in S1 in a continuous veneer carbonization line or veneer carbonization kiln, set the temperature to 200°C, and lightly carbonize for 3-15 minutes, while introducing inert gas or carbon dioxide gas during light carbonization.
[0029] The light carbonized layer (1) can be obtained;
[0030] S3: Coat the front and back sides of each light carbonized layer (1) treated in S2 with paraffin emulsion, and seal
[0031] Bag storage, health preservation for 24 hours;
[0032] S4: applying adhesive layers (2) to the paraffin wax light carbonized layers (1) processed in S3 respectively, and the gluing method is orthogonal gluing and then pressing, and curing, to finally form a light carbonized paraffin wax coated anti-deformation multilayer board with an odd number of layers;
[0033] Light carbonization steam spray process production methods include
[0034] S1: Peel the fast-growing poplar or other fast-growing materials into 2440×1220mm veneers with a thickness of 1-3mm;
[0035] S2: Directly use 100℃ steam on both sides of the poplar veneer or other fast-growing veneer described in S1
[0036] Spray for 5-10 minutes;
[0037] S3: Place the poplar veneer that has been steam-sprayed in S2 in a continuous veneer carbonization line or a carbonization kiln, set the temperature to 200°C, and perform light carbonization for 3-15 minutes. During the light carbonization, introduce inert gas or dioxygen.
[0038] The light carbonized layer (1) can be obtained by adding carbonizing gas;
[0039] S4: applying adhesive layers (2) to the steam spray carbonized layers (1) processed in S3 respectively, wherein the bonding method is orthogonal bonding followed by pressurization and curing, and finally forming a lightly carbonized steam spray anti-deformation multilayer board with an odd number of layers.
[0040] Compared with the existing technology, the advantages of this technology are:
[0041] 1. Through in-depth experimental verification, the light carbonization anti-deformation multilayer board of the present invention has significantly optimized and improved the performance in suppressing deformation compared with the multilayer board without carbonization treatment. This innovative achievement is mainly attributed to the light carbonization process's exquisite regulation of the wood microstructure and the effective release of the internal stress of the board, which significantly enhances the structural stability and dimensional retention ability of the board.
[0042] 2. In terms of the selection of adhesive layer materials, the present invention demonstrates a high degree of flexibility and adaptability. The adhesive layer can be made of adhesives with better strength or better waterproof performance, such as phenolic resin, polyurethane, etc., according to the specific application environment and functional requirements, to ensure the structural strength and durability of the multilayer board under different conditions. This feature not only broadens the application field of light carbonization anti-deformation multilayer boards, but also improves their performance in extreme environments, providing more reliable and diversified material solutions for industries such as construction and furniture manufacturing.
[0043] 3. Through the combination of light carbonization treatment and customized adhesive layer materials, the present invention achieves a significant leap in the anti-deformation performance of the multilayer board, while taking into account both aesthetics and practicality, bringing forward-looking technological innovation to the industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 The present invention provides a seven-layer light carbonization anti-deformation multilayer board with an overall structure schematic diagram.
[0045] Figure 2 It is a schematic diagram of an explosion of a seven-layer light carbonization anti-deformation multilayer board structure provided by the present invention.
[0046] The symbols in the figure represent:
[0047] 1. Light carbonization layer; 2. Adhesive layer; DETAILED DESCRIPTION
[0048] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0049] Example 1: (200°C, light carbonization for 9 minutes, full carbon assembly)
[0050] This embodiment is a light carbonized all-carbon type anti-deformation multilayer board and its manufacturing method. Single board preparation: Select fast-growing poplar wood as the raw material, use a rotary cutter to cut the wood into 2 mm thick single boards, these single boards are cut into 450 mm × 450 mm squares, and a total of 7 boards are prepared; light carbonization treatment: each layer of single board is sent to the continuous carbonization line through a conveyor belt. In this process, the single board is lightly carbonized at a temperature of 200°C for 9 minutes to obtain a light carbonized layer; glue coating treatment: after carbonization treatment, except for the outermost light carbonized layer, the remaining middle light carbonized layers are coated with phenolic resin adhesive on both sides, and the coating is The amount of glue is controlled at 270g / m2 to ensure that the light carbonized layer has sufficient strength and stability during bonding; assembly and hot pressing: the light carbonized layers after glue coating are stacked in an orthogonal manner to form a 7-layer light carbonized anti-deformation multilayer board, and then the assembly is placed in a press machine, the temperature is set to 130°C and the pressure is set to 1.2MPa, and a 15-minute hot pressing treatment is performed to solidify the phenolic resin. At the same time, the various layers of the multilayer board are tightly combined through heat and pressure to form a 7-layer light carbonized full-carbon anti-deformation multilayer board.
[0051] Example 2: (200°C, light carbonization for 9 minutes, 4 layers of light carbonization + 3 layers of non-carbonized interval carbon)
[0052] This embodiment is a 4-layer light carbonization + 3-layer non-carbonization spacer carbon type multilayer board with light carbonization and anti-deformation and its manufacturing method. The light carbonization multilayer board is assembled in the manner of the 1st and 7th layers, the 3rd and 5th layers are light carbonization layers, and the remaining 2, 4, and 6 are non-carbonization, that is, a 4 (light carbonization) + 3 (non-carbonization) spacer carbon anti-deformation multilayer board; the remaining methods are as described in Example 1, and finally a seven-layer structure of a light carbonization anti-deformation 4-layer light carbonization + 3 non-carbonization spacer carbon type multilayer board is formed.
[0053] Example 3: (200°C, light carbonization for 9 minutes, light carbonization of the upper and lower surfaces + non-carbonized surface carbon in the middle layer)
[0054] This embodiment is a surface carbon multilayer board with light carbonization of upper and lower surface layers and non-carbonization of middle layer and a manufacturing method thereof. The upper and lower surface layers are symmetrically assembled, the upper and lower surface layers are light carbonization layers, and the middle layer is all non-carbonization structure; the rest of the method is as described in Example 1, and finally a seven-layer structure of light carbon deformation-resistant surface carbon multilayer board is formed.
[0055] Example 4: (First, light carbonization for 9 minutes, then coating with paraffin emulsion)
[0056] This embodiment is a light charcoal anti-deformation paraffin-coated multilayer board and a manufacturing method thereof. The front and back sides of the carbonized layer of the light charcoal multilayer board are coated with paraffin emulsion respectively, and the board is stored in a sealed bag and cured for 4 hours. The remaining methods are as described in Example 1, and finally a seven-layer light charcoal anti-deformation paraffin-coated multilayer board is formed.
[0057] Example 5: (steam spraying first, then light carbonization for 9 minutes)
[0058] This embodiment is a light carbon anti-deformation steam spray multilayer board and its manufacturing method. Before light carbonization, the front and back sides of the poplar veneer are directly sprayed with 100°C steam for 10 minutes, and the rest of the method is as described in Example 1, and finally a seven-layer structure light carbon anti-deformation steam spray multilayer board is formed.
[0059] Comparative Example 1 (non-carbonized, urea-formaldehyde resin adhesive)
[0060] This comparative example is a non-carbonized multilayer board using urea-formaldehyde resin adhesive and its manufacturing method. Single board preparation: Select fast-growing poplar wood as raw material, use a rotary cutter to cut the wood into 2 mm thick single boards, these single boards are cut into 450 mm × 450 mm squares, and a total of 7 boards are prepared; no light carbonization treatment is performed, except for the outermost single board, the remaining middle layers are coated with urea-formaldehyde resin adhesive on both sides, and the amount of glue is controlled at 270g / m2 to ensure that the board has sufficient strength and stability during bonding; assembly and hot pressing: The glued single boards are stacked in an orthogonal manner to form a multilayer board with a 7-layer structure, and then placed in a press machine, set the temperature to 130°C and the pressure to 1.2MPa, and perform a 15-minute hot pressing treatment to solidify the urea-formaldehyde resin. At the same time, the various layers of the multilayer board are tightly combined by heat and pressure to form a multilayer board with a 7-layer structure.
[0061] Comparative Example 2 (Non-carbonized, phenolic resin adhesive)
[0062] This comparative example is a non-carbonized multilayer board using phenolic resin adhesive and a manufacturing method thereof, wherein the adhesive layer uses urea-formaldehyde resin adhesive, and the remaining steps and schemes are performed according to comparative example 1 to manufacture a multilayer board with a 7-layer structure.
[0063] The anti-deformation performance of the different light carbonized anti-deformation multilayer boards in the above embodiments was compared with the multilayer boards in the comparative examples. The test pieces were subjected to dimensional stability tests and mechanical property tests in accordance with the international standard GB / T 17657-2022. The experimental data results are shown in Tables 1, 2 and 3.
[0064] Table 1 Comparative test results of thickness changes of different types of light carbonized anti-deformation multilayer boards
[0065]
[0066] According to the data analysis in Table 1, the light carbonized anti-deformation multilayer board involved in this patent shows excellent dimensional stability. Whether in the environmental change from normal humidity to 85% high humidity or from normal humidity to 30% low humidity, its thickness change range is smaller than that of ordinary multilayer boards. Compared with ordinary multilayer boards, the dimensional stability of the light carbonized anti-deformation multilayer board is more than 90%, which shows that it has strong moisture resistance.
[0067] Table 2 Comparative test results of warpage changes of different types of light carbonized anti-deformation multilayer boards
[0068]
[0069] According to the detailed data analysis in Table 2, the light carbonized anti-deformation multilayer board developed by this patent shows significant advantages over ordinary multilayer boards. Whether in the transition from a normal humidity environment to a high humidity condition of up to 85% humidity, or in a low humidity environment with a sudden drop to 30% humidity, the change in its warpage is significantly lower than that of a conventional multilayer board, demonstrating its excellent humidity adaptability and stability.
[0070] Table 3 Comparative test results of mechanical properties of different types of light carbonized anti-deformation multilayer boards
[0071]
[0072]
[0073] According to the in-depth analysis of Table 3, the light carbonized anti-deformation multilayer board developed by this patent shows mechanical properties comparable to those of ordinary plywood, without obvious performance disadvantages. Light carbonization technology ensures the mechanical strength of the material while maintaining the mechanical properties of wood, opens up new ways for the sustainable use and environmentally friendly design of artificial boards, and provides a high-quality material choice with both performance and ecological value for the construction and furniture manufacturing industries.
Claims
1. A light carbonization anti-deformation multilayer board, comprising a light carbonization layer (1) and a glue layer (2), characterized in that: The substrate of the light carbonized layer (1) is sprayed with high-temperature steam before carbonization or coated with a waterproofing agent after carbonization, or is treated with a combination of the two or is left untreated.
2. The light carbonization anti-deformation multilayer board according to claim 1, characterized in that: The light carbonization anti-deformation multi-layer plate is assembled in the form of full carbon, interval carbon, or surface carbon.
3. The light carbonization anti-deformation multilayer board according to claim 2, characterized in that: The full carbon of the lightly carbonized anti-deformation multilayer board is a multilayer lightly carbonized structure assembled into 3 layers, 5 layers, 7 layers, or an odd-numbered multilayer board; the interval carbon is a multilayer lightly carbonized structure assembled in an interval symmetrical manner; the surface carbon includes at least two layers of lightly carbonized structures that respectively constitute the upper and lower surface layers of the multilayer board.
4. The light carbonization anti-deformation multilayer board according to claim 1, characterized in that: The carbonization temperature of the light carbonization layer is 190-220° C., and the carbonization time is 3-15 minutes.
5. The light carbonization anti-deformation multilayer board according to claim 1, characterized in that: The adhesive layer (2) includes but is not limited to urea-formaldehyde resin, phenol-formaldehyde resin and melamine glue or hydrophobic adhesive.
6. A method for manufacturing a light carbonized anti-deformation multilayer board according to claims 1-5, characterized in that: It covers the full carbon assembly process production mode, the interval carbon assembly process production mode, the surface carbon assembly process production mode, the paraffin coating process production mode, and the steam spray process production mode, including the following steps: The light carbonization full carbon assembly process production methods include: S1: Peel the fast-growing poplar or other fast-growing wood into 2440×1220mm veneers with a veneer thickness of 1-3mm and a veneer thickness of 1-3mm; S2: placing the poplar veneer described in S1 in a continuous veneer carbonization line or a veneer carbonization kiln, setting the temperature to 200° C., lightly carbonizing for 3-15 minutes, and introducing inert gas or carbon dioxide gas during the light carbonization to obtain the lightly carbonized layer (1); S3: brushing the lightly carbonized layers (1) treated in S2 with adhesive layers (2) respectively, and the gluing method is orthogonal gluing and then pressurizing, and curing, and finally forming a lightly carbonized full-carbon anti-deformation multilayer board with an odd number of layers; The light carbonization interval assembly process production methods include: S1: Peel the fast-growing poplar or other fast-growing wood into 2440×1220mm veneers with a thickness of 1-3mm; S2: placing the poplar veneer described in S1 in a continuous veneer carbonization line or a veneer carbonization kiln, setting the temperature to 200° C., lightly carbonizing for 3-15 minutes, and introducing inert gas or carbon dioxide gas during the light carbonization to obtain the lightly carbonized layer (1); S3: brushing the lightly carbonized layer (1) treated in S2 with a glue layer (2) respectively, and assembling the blanks in an interval-type symmetrical manner, wherein the first layer is the lightly carbonized layer (1), the second layer is not carbonized, the third layer is the lightly carbonized layer (1), and so on to form an interval-type symmetrical blank assembly structure; S4: orthogonally gluing the symmetrical blank structure completed in S3 and then applying pressure to solidify it, and finally forming a light carbonized interval anti-deformation multilayer board with an odd number of layers; Light carbonization surface carbon assembly process production methods include S1: Peel the fast-growing poplar or other fast-growing wood into 2440×1220mm veneers with a thickness of 1-3mm; S2: placing the poplar veneer described in S1 in a continuous veneer carbonization line or a veneer carbonization kiln, setting the temperature to 200° C., lightly carbonizing for 3-15 minutes, and introducing inert gas or carbon dioxide gas during the light carbonization to obtain the lightly carbonized layer (1); S3: brushing the lightly carbonized layer (1) treated in S2 with a glue layer (2) respectively, and assembling the blanks symmetrically according to the upper and lower surface layers, wherein the upper and lower surface layers are the lightly carbonized layer (1), and the remaining middle layers are all uncarbonized structures; S4: orthogonally gluing the surface symmetrical assembly structure completed in S3 and then applying pressure and curing, and finally forming a lightly carbonized surface carbon anti-deformation multilayer board with an odd number of layers; Light carbonized paraffin coating process production methods include S1: Peel the fast-growing poplar or other fast-growing wood into 2440×1220mm veneers with a thickness of 1-3mm; S2: placing the poplar veneer described in S1 in a continuous veneer carbonization line or a veneer carbonization kiln, setting the temperature to 200° C., lightly carbonizing for 3-15 minutes, and introducing inert gas or carbon dioxide gas during the light carbonization to obtain the lightly carbonized layer (1); S3: coating the front and back sides of each light carbonized layer (1) treated in S2 with paraffin emulsion respectively, storing in a sealed bag, and curing for 24 hours; S4: applying adhesive layers (2) to the paraffin wax light carbonized layers (1) processed in S3 respectively, and the gluing method is orthogonal gluing and then pressing, and curing, to finally form a light carbonized paraffin wax coated anti-deformation multilayer board with an odd number of layers; Light carbonization steam spray process production methods include S1: Peel the fast-growing poplar or other fast-growing wood into 2440×1220mm veneers with a thickness of 1-3mm; S2: directly spray the front and back sides of the poplar veneer or other fast-growing veneer described in S1 with 100°C steam for 5-10 minutes; S3: placing the poplar veneer that has been steam-sprayed in S2 in a continuous veneer carbonization line or a carbonization kiln, setting the temperature to 200° C., and lightly carbonizing for 3-15 minutes, while introducing an inert gas or carbon dioxide gas during the light carbonization, thereby obtaining the lightly carbonized layer (1); S4: applying adhesive layers (2) to the steam spray carbonized layers (1) processed in S3 respectively, wherein the bonding method is orthogonal bonding followed by pressurization and curing, and finally forming a lightly carbonized steam spray anti-deformation multilayer board with an odd number of layers.
Citation Information
Patent Citations
Method for preparing eucalyptus structural wood
CN102554998A
Manufacture method of solid-wood water preventing material
CN103056942A
Carbonized plywood and manufacturing method thereof
CN103692505A
Cotton-wood hot-wax drying and high temperature heat treatment integrated technology
CN107520932A
Micro-carbonization method for solid wood floor
CN108972813A
Cited By
Carbonized floor and lamination preparation method thereof
CN121061980A
A carbonized flooring and a laminating method thereof
CN121061980B