Spherical rare earth oxide resonance unit with controllable size and composition and cascade preparation method and application of spherical rare earth oxide resonance unit
By pre-adding seed solution and controlling the reaction conditions, the size and component controllability problems in the preparation of submicron-scale spherical rare earth oxide resonant units are solved, and an efficient and low-cost cascade preparation method is realized, which is suitable for a variety of Optical and sensing applications.
Patent Information
- Application Number
- CN202411105885.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to accurately prepare spherical rare earth oxide resonant units with controllable size and components on the submicron scale, resulting in limited application stability and performance in high temperature environments.
By pre-adding seed crystal solution, the reaction between the yttrium salt solution and the seed precipitant is controlled, and the conditions of metal salt solution and alkaline precipitant are combined to realize the cascade preparation of spherical rare earth oxide resonant units, avoiding the explosive nucleation process. Ensure controllability of size and components.
The preparation of spherical rare earth oxide resonant units with high spherical morphology and uniform size distribution in the range of 0.1-1μm was achieved, which reduced production costs, was suitable for industrial applications, and showed excellent performance in the fields of disordered superstructures, photonic crystals, etc.
Smart Images

Figure CN118993129A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical ceramics and functional ceramic materials, and specifically relates to a spherical rare earth oxide resonance unit with controllable size and composition, and a cascade preparation method and application thereof. Background Art
[0002] The resonant structure manipulates the propagation behavior of light by carefully designing the morphology, components and assembly structure of the micro-nano resonant unit. It has strong frequency selectivity and can produce a series of special optical resonance effects to achieve efficient reflection, transmission and absorption of incident light, such as disordered superstructures, photonic crystals, metasurfaces, etc. It is particularly significant when the characteristic scale of the resonant unit is close to the wavelength of light. Its back reflection efficiency is high, and it can achieve high reflection or high emission characteristics for wavelengths in a certain frequency band. The highly symmetrical spherical resonant unit is isotropic, which can effectively reduce the design complexity and processing difficulty. Rare earth oxides represented by yttrium oxide are abundant rare earth sesquioxide resources in my country. They have a high melting point (2430℃), dielectric constant (12-14), refractive index (n=1.89 / 1050nm), thermal conductivity (13.6W), chemical stability, and low phonon energy (550cm -1), wide band gap (about 5.8eV), wide optical transparency band, etc., making it an ideal candidate material for optical scattering resonance units. Submicron-scale resonance units are close to the wavelengths of widely used ultraviolet, visible and near-infrared light. Researchers are actively trying to achieve specific resonance efficiency in this band through structural design. However, the cutting-edge structural models and theoretical mechanisms need further experimental verification due to the lack of precise preparation of submicron-scale spherical resonance units. Submicron spherical rare earth oxide resonance units with controllable size and composition can accommodate the rich emission energy levels of most rare earth ions, show a resonant light scattering enhancement effect, and produce narrow-band fluorescence with high color purity and conversion efficiency. They are widely used in plasma display panel devices, lighting sources, information display and transmission, temperature sensor devices, solar photovoltaic conversion, biomarkers and imaging probes. Submicron spherical rare earth oxide resonance units with controllable size and composition can be used for photothermal radiation in high-temperature environments. Their size and composition directly affect the application stability and performance in photothermal radiation environments. Submicron spherical rare earth oxide resonant units with controllable size and composition also play an important role in catalysis, sensor materials, biomedicine, molecular testing and other fields due to the precise adjustability of their resonant units and structures. Especially in optical applications, high refractive index rare earth oxide submicron spheres can simultaneously excite electric dipole resonance and magnetic dipole resonance, causing rich resonance effects, such as Mie resonance and Fano resonance. Submicron spherical rare earth oxide resonant units of different sizes and compositions can significantly change the intensity and polarization state of scattered light, realize multi-parameter regulation of light fields in a wide band range, and can be widely used in nonlinear effect enhancement, one-way scattering, biosensing and other fields. Submicron spherical rare earth oxide resonant units with controllable size and composition can also effectively construct photonic crystals with periodic structures, generate photonic band gaps of specific frequencies, and manipulate the propagation behavior of light. Therefore, submicron spherical rare earth oxide resonant units with controllable size and composition have broad market prospects and are of great significance to the high-end manufacturing of my country's industry.
[0003] At present, the preparation of submicron-scale spherical rare earth oxide resonance units mainly includes spray pyrolysis, sol-gel method, hydrothermal method, precipitation method and other methods. The resonance units prepared by spray pyrolysis and sol-gel method have poor sphericity and a wide size distribution range, which cannot be applied to the precise construction of resonance structures. The hydrothermal method requires a high temperature and high pressure environment, which is costly and limits its application in industrial production. The precipitation method is a green, simple and low-cost method for preparing submicron spherical rare earth oxide resonance units. The resonance unit prepared by the urea homogeneous precipitation method has good sphericity, but due to the explosive nucleation caused by the instantaneous thermal decomposition of urea, the size is small and the components are segregated, which makes it difficult to achieve controllable preparation at the submicron scale. Although the microwave or hydrothermal assisted urea precipitation method can shorten the reaction time, it still cannot solve the problem of controllable preparation of submicron scale size and components. Therefore, there is still a lack of an effective cascade preparation method for spherical rare earth oxide resonance units with submicron scale size and controllable components. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a cascade preparation method for spherical rare earth oxide resonance units with controllable size and composition. The method greatly avoids the explosive nucleation process by adding a seed solution in advance, and the reaction product of the rare earth salt solution and the seed precipitant can be directly used for growth, and there is no problem of concentration segregation in the growth monomer. By adjusting the amount of seed solution, the type and concentration of the metal salt solution and the alkaline precipitant and other conditions, the number of seeds and the growth process are controlled to obtain spherical rare earth oxide resonance units of different sizes and components. The method of the present invention does not require special instruments and equipment, uses water as a medium, does not require organic reagents or emulsifiers, is low in cost, and is easy to operate. The spherical rare earth oxide resonance unit can be applied to disordered superstructures, photonic crystals, metasurface materials, sensor devices, solar photovoltaic conversion, biomedical detection, radiation cooling, high-energy laser protection and other fields. Compared with other methods for preparing spherical oxides, this method can significantly regulate the size and composition of spherical rare earth oxide resonance units at the submicron scale, and can achieve the preparation of spherical rare earth oxide resonance units with controllable size and composition in the range of 0.1-1μm, high sphericity, and a size polydispersity coefficient of less than 0.1.
[0005] The technical solution of the present invention is as follows:
[0006] The invention discloses a spherical rare earth oxide resonance unit with controllable size and composition. The yttrium salt solution and a seed crystal precipitant are first reacted to obtain a seed crystal solution. The seed crystal solution is introduced into a crystal nucleus, and a metal salt solution and an alkaline precipitant are added to grow the crystal nucleus. The spherical rare earth oxide resonance units with different sizes and compositions are obtained by controlling the amount of the seed crystal solution, the type and concentration of the metal salt solution and the alkaline precipitant.
[0007] The spherical rare earth oxide resonance unit has a high sphericity, a particle size range of 0.1-1 μm, the particle size is adjustable within the range, and is uniformly distributed, with a particle size polydispersity coefficient of less than 0.1.
[0008] In one embodiment of the present invention, preferably, the yttrium salt solution is yttrium nitrate, yttrium sulfate or yttrium halide solution; the seed precipitant is one or more of sodium hydroxide, potassium hydroxide, ammonia water, urea, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, formic acid, acetic acid, oxalic acid, butyric acid, valeric acid, hexanoic acid, octanoic acid, heptanoic acid, lauric acid, stearic acid, oleic acid, citric acid or ascorbic acid.
[0009] In one embodiment of the present invention, preferably, the metal salt solution is yttrium salt, or one or more of yttrium salt and other metal salts, and the other metal salts are scandium salts, lanthanum salts, cerium salts, praseodymium salts, neodymium salts, samarium salts, europium salts, gadolinium salts, terbium salts, dysprosium salts, thulium salts or ytterbium salts; and the metal salt is nitrate, sulfate or halide.
[0010] In one embodiment of the present invention, preferably, the molar ratio of the yttrium salt to the other metal salt is 2:1-100:1.
[0011] In one embodiment of the present invention, preferably, the alkaline precipitant is sodium hydroxide, potassium hydroxide, ammonia water or urea.
[0012] The present invention also discloses a cascade preparation method of the above-mentioned spherical rare earth oxide resonance unit with controllable size and composition, which is characterized by comprising the following steps:
[0013] (1) preparing a seed solution: mixing a yttrium salt solution and a seed precipitant, reacting at 0-20° C. for 6-12 hours to obtain a seed solution, wherein the concentration of the yttrium salt solution is 0.5-20 mmol / L, and the molar ratio of the yttrium salt solution to the seed precipitant is 1:1-1:20;
[0014] (2) Cascade preparation of spherical rare earth oxide resonance units: disperse the seed solution in a metal salt solution, add an alkaline precipitant and react at 40-100°C; or disperse the seed solution in water, dropwise add a metal salt solution and a precipitant at 40-100°C, react, cool to room temperature after the reaction, wash by centrifugation, dry and then heat-treat to obtain a spherical rare earth oxide resonance unit.
[0015] In one embodiment of the present invention, preferably, in step (2), when the spherical rare earth oxide resonance unit is prepared by cascading, a seed solution is selected and dispersed in a metal salt solution, and an alkaline precipitant is added to react at 40-100°C, the volume ratio of the seed solution to the metal salt solution is 1:50-1:500, the metal salt concentration is 5-100 mmol / L, the molar ratio of the metal salt to the alkaline precipitant is 1:2-1:50, and the reaction time is 2-24h.
[0016] In one embodiment of the present invention, preferably, in step (2), when the spherical rare earth oxide resonance unit is prepared by cascading, a seed solution is selected and dispersed in water, and a metal salt solution and a precipitant are added dropwise at 40-100°C to react, the volume ratio of the seed solution to the metal salt solution is 1:50-1:500, the metal salt concentration is 0.01-0.5 mol / L, the molar ratio of the metal salt to the alkaline precipitant is 1:2-1:10, the dropping speed is 5-20 mL / h, and the dropping time is 2-72 h.
[0017] In one embodiment of the present invention, preferably, in step (2), the drying temperature is 70-200° C., the drying time is 4-24 h, the heat treatment temperature is 600-1200° C., and the heat treatment time is 2-6 h.
[0018] The present invention also discloses the application of the above-mentioned spherical rare earth oxide resonance unit with controllable size and composition in disordered superstructures, photonic crystals, supersurface materials, sensor devices, solar photovoltaic conversion, biomedical detection, radiation cooling, and high-energy laser protection materials.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The cascade preparation method constructed by the present invention using a pre-synthesized seed solution greatly avoids the explosive nucleation process, which is conducive to the growth of spherical rare earth oxide resonance units with controllable size and composition; the preparation of spherical rare earth oxide resonance units by the present invention can accurately control the size and composition of the spherical rare earth oxide resonance units by changing the amount of seed solution, the type, concentration, reaction time and other conditions of the metal salt solution and precipitant; the obtained spherical rare earth oxide resonance units are controllable in size within the range of 0.1-1 μm, have no agglomeration after heat treatment, have high sphericity, smooth surface morphology, narrow size distribution, and a size polydispersity coefficient of less than 0.1;
[0021] (2) The present invention uses water as a solvent, and does not use an organic solvent, dispersant or emulsifier, which is green and environmentally friendly, and avoids the problem of environmental pollution and high cost caused by organic solvents as solvents; the method of the present invention is simple and easy to operate, has low requirements for instruments and equipment, has a controllable preparation process, high synthesis efficiency, and is suitable for large-scale production;
[0022] (3) The spherical rare earth oxide resonance unit prepared by the method of the present invention has a structural composition similar to that of macroscopic matter and has stable performance. It can be applied to disordered superstructures, photonic crystals, metasurface materials, sensor devices, solar photovoltaic conversion, biomedical detection, radiation cooling, high-energy laser protection and other fields. The cascade preparation method provides a new approach for spherical oxide resonance units with controllable size and composition. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The scanning electron microscope images of the spherical rare earth oxide resonance unit precursors prepared in Examples 1 to 9 of the method of the present invention, wherein (a) is the 0.15±0.01μm spherical lanthanum-doped yttrium oxide resonance unit precursor prepared in Example 5, (b) is the 0.27±0.01μm spherical yttrium oxide resonance unit precursor prepared in Example 2, (c) is the 0.36±0.02μm spherical cerium-doped yttrium oxide resonance unit precursor prepared in Example 6, (d) is the 0.45±0.02μm spherical praseodymium-doped yttrium oxide resonance unit precursor prepared in Example 7, and ( e) is the 0.54±0.02μm spherical samarium-doped yttrium oxide resonance unit precursor prepared in Example 1, (f) is the 0.61±0.03μm spherical europium-doped yttrium oxide resonance unit precursor prepared in Example 4, (g) is the 0.72±0.04μm spherical gadolinium-doped yttrium oxide resonance unit precursor prepared in Example 3, (h) is the 0.81±0.04μm spherical thulium-doped yttrium oxide resonance unit precursor prepared in Example 8, (i) is the 0.95±0.05μm spherical ytterbium-doped yttrium oxide resonance unit precursor prepared in Example 9;
[0024] Figure 2 This is a size distribution diagram of the spherical samarium-doped yttrium oxide resonance unit precursor prepared in Example 1 of the method of the present invention;
[0025] Figure 3 The X-ray diffraction pattern of the spherical samarium-doped yttrium oxide resonance unit precursor prepared in Example 1 of the method of the present invention;
[0026] Figure 4 The X-ray diffraction pattern of the spherical samarium-doped yttrium oxide resonance unit precursor after heat treatment of Example 1;
[0027] Figure 5 This is a scanning electron microscope image of the spherical yttrium oxide resonance unit precursor of Example 2, which is a spherical yttrium oxide submicron sphere after heat treatment;
[0028] Figure 6 This is a scanning electron microscope image of the spherical praseodymium-doped yttrium oxide resonance unit obtained in Example 7 after self-assembly. DETAILED DESCRIPTION
[0029] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0030] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.
[0031] Example 1
[0032] Embodiment 1 of the present invention provides a spherical rare earth oxide resonance unit with controllable size and composition and a cascade preparation method thereof, which specifically comprises the following steps:
[0033] Yttrium nitrate solution and sodium hydroxide solution (yttrium nitrate concentration is 5 mmol / L, and the molar ratio of yttrium nitrate to sodium hydroxide is 1:2) are mixed evenly, and reacted at 0°C for 12 hours to obtain a seed solution. 1 mL of the seed solution is dispersed in 200 mL of 10 mmol / L metal salt solution, and the molar ratio of yttrium nitrate to samarium nitrate in the metal salt solution is 20:1. Urea (the molar ratio of metal salt to urea is 1:10) is added and mixed evenly, and then the temperature is raised to 90°C and reacted for 6 hours. After the reaction is completed, it is naturally cooled to room temperature, and centrifuged and washed to obtain a spherical samarium-doped yttrium oxide resonance unit precursor. After drying at 70°C for 12 hours, the spherical samarium-doped yttrium oxide resonance unit is obtained by heat treatment at 1200°C for 4 hours.
[0034] The SEM image of the obtained spherical samarium-doped yttrium oxide resonant unit precursor is shown in Figure 1 As shown in (e), the prepared spherical samarium-doped yttrium oxide resonance unit precursor has a high sphericity, a size of 0.54±0.02 μm, and a uniform size distribution with a size polydispersity coefficient of less than 0.1, as shown in Figure 2 The X-ray diffraction pattern of the spherical samarium-doped yttrium oxide resonance unit precursor is shown in Figure 3 As shown, it is shown that the precursor exhibits an amorphous structure due to its main component being basic carbonate, which transforms into tetragonal samarium-doped yttrium oxide after heat treatment, e.g. Figure 4 As shown, the spherical samarium-doped yttrium oxide resonance unit after heat treatment has a higher crystallinity.
[0035] Example 2
[0036] Embodiment 2 of the present invention provides a spherical rare earth oxide resonance unit with controllable size and composition and a cascade preparation method thereof, which specifically comprises the following steps:
[0037] After the yttrium chloride solution and the acetic acid solution (the yttrium chloride concentration is 20mmol / L, and the molar ratio of yttrium chloride to acetic acid is 1:10) are mixed evenly, the mixture is reacted at 20°C for 6h to obtain a seed solution, 4mL of the seed solution is dispersed in 200mL of a 40mmol / L yttrium nitrate solution, urea (the molar ratio of yttrium nitrate to urea is 1:50) is added and mixed evenly, and the mixture is heated to 100°C and reacted for 2h. After the reaction is completed, the mixture is naturally cooled to room temperature, and the mixture is centrifuged and washed to obtain a spherical yttrium oxide resonance unit precursor. After drying at 100°C for 4h, the mixture is heat treated at 600°C for 4h to obtain a spherical yttrium oxide resonance unit.
[0038] The SEM image of the obtained spherical yttrium oxide resonance unit precursor is as follows: Figure 1 As shown in (b), the prepared spherical yttrium oxide resonance unit precursor has a high sphericity, a size of 0.27±0.01μm, and a uniform size distribution, with a size polydispersity coefficient of less than 0.1. The SEM image of the obtained spherical yttrium oxide resonance unit after heat treatment is as follows Figure 5 As shown, the size changes slightly after heat treatment and the sphericity is well maintained.
[0039] Example 3
[0040] The present invention implements a spherical rare earth oxide resonance unit with controllable size and composition and a cascade preparation method thereof, which specifically comprises the following steps:
[0041] After the yttrium nitrate solution and the sodium carbonate solution (the yttrium nitrate concentration is 0.5mmol / L, and the molar ratio of yttrium nitrate to carbonate is 1:1) are evenly mixed, the mixture is reacted at 10°C for 12h to obtain a seed solution, 2mL of the seed solution is dispersed in 100mL of water and the temperature is raised to 80°C, and 0.1mol / L of a metal salt solution and 0.2mol / L of a sodium hydroxide solution are continuously added at a rate of 5mL / h, the molar ratio of yttrium chloride to gadolinium chloride in the metal salt solution is 50:1, and the addition time is 20h. After the reaction is completed, the mixture is naturally cooled to room temperature, centrifuged and washed to obtain a spherical gadolinium-doped yttrium oxide resonance unit precursor, dried at 80°C for 6h, and heat treated at 800°C for 6h to obtain a spherical gadolinium-doped yttrium oxide resonance unit.
[0042] The SEM image of the obtained spherical gadolinium-doped yttrium oxide resonant unit precursor is as follows: Figure 1 As shown in (g), the prepared spherical gadolinium-doped yttrium oxide resonance unit precursor has a high sphericity, a size of 0.72±0.04 μm, and a uniform size distribution with a size polydispersity coefficient of less than 0.1.
[0043] Example 4
[0044] Embodiment 4 of the present invention provides a spherical rare earth oxide resonance unit with controllable size and composition and a cascade preparation method thereof, which specifically comprises the following steps:
[0045] The yttrium sulfate solution and tetramethylammonium hydroxide solution (yttrium sulfate concentration is 10mmol / L, and the molar ratio of yttrium sulfate to tetramethylammonium hydroxide is 1:1) are mixed evenly, and then reacted at 20°C for 8h to obtain a seed solution. 1mL of the seed solution is dispersed in 50mL of water and heated to 60°C. 0.01mol / L of metal salt solution and 0.1mol / L of ammonia solution are continuously added at a rate of 20mL / h. The molar ratio of yttrium sulfate to europium sulfate in the metal salt solution is 80:1. The addition time is 36h. After the reaction is completed, it is naturally cooled to room temperature, centrifuged and washed to obtain a spherical europium-doped yttrium oxide resonance unit precursor, dried at 200°C for 4h, and heat treated at 800°C for 6h to obtain a spherical europium-doped yttrium oxide resonance unit.
[0046] The SEM image of the obtained spherical europium-doped yttrium oxide resonant unit precursor is as follows: Figure 1 As shown in (f), the prepared spherical europium-doped yttrium oxide resonance unit precursor has a high sphericity, a size of 0.61±0.03 μm, and a uniform size distribution with a size polydispersity coefficient of less than 0.1.
[0047] Embodiment 5-7
[0048] In Example 2, the seed solution was dispersed in 200 mL of 20 mmol / L, 60 mmol / L and 80 mmol / L metal salt solutions, respectively. The metal salt solutions were yttrium nitrate and lanthanum nitrate mixed solution (molar ratio of 10:1), yttrium nitrate and cerium nitrate mixed solution (molar ratio of 50:1), and yttrium nitrate and praseodymium nitrate mixed solution (molar ratio of 100:1). Spherical lanthanum, cerium, and praseodymium doped yttrium oxide resonance unit precursors with sizes of 0.15 ± 0.01 μm, 0.36 ± 0.02 μm, and 0.45 ± 0.02 μm were prepared, respectively. The scanning electron microscope images of the obtained spherical lanthanum, cerium, and praseodymium doped yttrium oxide resonance unit precursors are shown in FIG. Figure 1 As shown in (a), (c), and (d), the prepared spherical lanthanum, cerium, and praseodymium doped yttrium oxide resonance unit precursors have high sphericity and uniform size distribution, and the size polydispersity coefficient is less than 0.1, as shown in Figure 6 As shown, Figure 1 (d) The spherical praseodymium-doped yttria resonant unit precursor can self-assemble into a photonic crystal structure, indicating that its size is highly uniform.
[0049] Embodiment 8-9
[0050] In Example 3, the metal salt solution and the sodium hydroxide solution are continuously added for 40 hours and 60 hours, and the metal salt solutions are respectively a mixed solution of yttrium nitrate and thulium nitrate (molar ratio of 60:1) and a mixed solution of yttrium nitrate and ytterbium nitrate (molar ratio of 80:1). Spherical thulium and ytterbium doped yttrium oxide resonance unit precursors with sizes of 0.81±0.04μm and 0.95±0.05μm can be prepared respectively. The scanning electron microscope images of the obtained spherical thulium and ytterbium doped yttrium oxide resonance unit precursors are shown in FIG. Figure 1 As shown in (h) and (i), the prepared spherical thulium and ytterbium doped yttrium oxide resonance unit precursors have high sphericity and uniform size distribution, and the size polydispersity coefficient is less than 0.1.
[0051] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A spherical rare earth oxide resonant unit with controllable size and composition, It is characterized in that First, a yttrium salt solution and a seed crystal precipitant are reacted to obtain a seed crystal solution; the seed crystal solution is introduced into a crystal nucleus, and a metal salt solution and an alkaline precipitant are added to grow the crystal nucleus, and spherical rare earth oxide resonance units of different sizes and components are obtained by controlling the amount of the seed crystal solution, the type and concentration of the metal salt solution and the alkaline precipitant; The spherical rare earth oxide resonance unit has a high sphericity, a particle size range of 0.1-1 μm, the particle size is adjustable within the range, and is uniformly distributed, and the particle size polydispersity coefficient is less than 0.
1.
2. The spherical rare earth oxide resonance unit with controllable size and composition according to claim 1, It is characterized in that The yttrium salt solution is yttrium nitrate, yttrium sulfate or yttrium halide solution; the seed precipitant is one or more of sodium hydroxide, potassium hydroxide, ammonia water, urea, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, formic acid, acetic acid, oxalic acid, butyric acid, valeric acid, hexanoic acid, octanoic acid, heptanoic acid, lauric acid, stearic acid, oleic acid, citric acid or ascorbic acid.
3. The spherical rare earth oxide resonance unit with controllable size and composition according to claim 1, It is characterized in that The metal salt solution is yttrium salt, or one or more of yttrium salt and other metal salts, and the other metal salts are scandium salts, lanthanum salts, cerium salts, praseodymium salts, neodymium salts, samarium salts, europium salts, gadolinium salts, terbium salts, dysprosium salts, thulium salts or ytterbium salts; the metal salt is nitrate, sulfate or halide.
4. The spherical rare earth oxide resonance unit with controllable size and composition according to claim 3, It is characterized in that The molar ratio of the yttrium salt to other metal salts is 2:1-100:
1.
5. The spherical rare earth oxide resonance unit with controllable size and composition according to claim 1, It is characterized in that The alkaline precipitant is sodium hydroxide, potassium hydroxide, ammonia water or urea.
6. A cascade preparation method of a spherical rare earth oxide resonance unit with controllable size and composition as claimed in any one of claims 1 to 5, It is characterized in that The following steps are involved: (1) preparing a seed solution: mixing a yttrium salt solution and a seed precipitant, reacting at 0-20° C. for 6-12 hours to obtain a seed solution, wherein the concentration of the yttrium salt solution is 0.5-20 mmol / L, and the molar ratio of the yttrium salt solution to the seed precipitant is 1:1-1:20; (2) Cascade preparation of spherical rare earth oxide resonance units: disperse the seed solution in a metal salt solution, add an alkaline precipitant and react at 40-100°C; or disperse the seed solution in water, dropwise add a metal salt solution and a precipitant at 40-100°C, react, cool to room temperature after the reaction, wash by centrifugation, dry and then heat-treat to obtain a spherical rare earth oxide resonance unit.
7. The cascade preparation method of the spherical rare earth oxide resonance unit with controllable size and composition according to claim 6, It is characterized in that In step (2), when the spherical rare earth oxide resonance unit is prepared by cascading, a seed solution is selected and dispersed in a metal salt solution, and an alkaline precipitant is added to react at 40-100°C, the volume ratio of the seed solution to the metal salt solution is 1:50-1:500, the metal salt concentration is 5-100 mmol / L, the molar ratio of the metal salt to the alkaline precipitant is 1:2-1:50, and the reaction time is 2-24h.
8. The method for preparing the spherical rare earth oxide resonance unit with controllable size and composition according to claim 6, It is characterized in that In step (2), when the spherical rare earth oxide resonance unit is prepared by cascading, a seed solution is selected and dispersed in water, and a metal salt solution and a precipitant are added dropwise at 40-100° C. to react, the volume ratio of the seed solution to the metal salt solution is 1:50-1:500, the metal salt concentration is 0.01-0.5 mol / L, the molar ratio of the metal salt to the alkaline precipitant is 1:2-1:10, the dropping speed is 5-20 mL / h, and the dropping time is 2-72 h.
9. The cascade preparation method of the spherical rare earth oxide resonance unit with controllable size and composition according to claim 7 or 8, It is characterized in that In step (2), the drying temperature is 70-200°C, the drying time is 4-24h, the heat treatment temperature is 600-1200°C, and the heat treatment time is 2-6h.
10. Application of the spherical rare earth oxide resonance unit with controllable size and composition as described in any one of claims 1 to 5 in disordered superstructures, photonic crystals, metasurface materials, sensor devices, solar photovoltaic conversion, biomedical detection, radiation cooling, and high-energy laser protection materials.
Citation Information
Cited By
Preparation method of high-purity sphere-like nano yttrium oxide powder
CN120081407A