Method for producing electrolyte-grade ammonium metavanadate by taking sodium polyvanadate as raw material
Through the leaching method of sodium polyvanadate and sodium hydroxide and the removal of impurities of sodium sulfide, combined with aluminum sulfate and magnesium sulfate treatment, the content and recovery of ammonium metavanadate were successfully improved, and the production process in the prior art was solved The problems of long, high energy consumption and high cost have achieved efficient and low-cost high-quality ammonium metavanadate production.
Patent Information
- Application Number
- CN202411089537.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
The existing methods for producing ammonium metavanadate have long processes, large energy consumption, low recovery rate, high production costs, low vanadium pentoxide content and high impurities, which cannot meet the dual needs of high-end customers for high quality and low price.
Using sodium polyvanadate as raw material, vanadium pentoxide is mixed with water by sodium hydroxide leaching method, heated to 50°C and dissolved, sodium sulfide is added to remove impurities, and then aluminum sulfate and magnesium sulfate are added to adjust the pH value, and settled for 48 hours. After filtering, a vanadium precipitant agent was added to deposit, washed with pure water and recovered with vanadium ion exchange, and finally obtained a high purity ammonium metavanadate.
It has achieved efficient production with a leachate rate of more than 98.5%, and the vanadium pentoxide content exceeds 99.80%, which simplifies the process flow, reduces energy consumption and production costs, and meets the needs of high-end customers for high-quality products.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nonferrous metallurgy, and particularly relates to a method for producing electrolyte-grade ammonium metavanadate by taking sodium polyvanadate as a raw material. Background Art
[0002] Vanadium is a transition metal element, mainly used as an additive in the metallurgical industry to produce high-strength alloy steel containing vanadium. At the same time, some new vanadium-containing alloys have also been promoted. Vanadium-containing titanium alloys can be used in the aviation and aerospace industries, initially used in aircraft engines and later used in fuselages. Vanadium-containing structural materials in the nuclear industry can meet the performance requirements of reactor structural materials in the nuclear industry. Vanadium-containing superconducting materials are preferred as efficient superconducting materials by the United States, Japan and other countries. Vanadium-containing new energy materials, vanadium-based new hydrogen solid materials, vanadium-based catalysts, vanadium-containing optical materials, vanadium-containing nanomaterials, vanadium-containing pigments and vanadium-containing biomedicine have also made great progress.
[0003] Renewable energy generation (such as wind power and solar power generation) is affected by natural environment and geographical conditions such as day and night alternation and seasonal changes. The power output is discontinuous, unstable and uncontrollable, which has a serious impact on the safe and stable operation of the power grid. In order to alleviate the impact of renewable energy generation on the power grid and improve the power grid's acceptance of renewable energy generation, it is necessary to use large-capacity energy storage devices to modulate the amplitude and frequency, smooth the output, and plan and track the power generation to improve the continuity, stability and controllability of renewable energy generation. Therefore, large-scale energy storage technology is a key bottleneck technology to solve the popularization and application of renewable energy generation. All-vanadium liquid flow batteries have the characteristics of good safety, independent design of output power and energy storage capacity, high and uniform single-cell stack power, flexible and easy expansion of energy storage system design, etc. They are suitable for energy storage ranges with output power ranging from several kW to hundreds of MW and energy storage capacity ranging from hundreds of kWh to hundreds of MWh. In the field of large-scale fixed energy storage applications in power systems, considering the safety of energy storage systems, the cost-effectiveness of the life cycle and the environmental load, all-vanadium liquid flow battery energy storage technology has important market prospects in the power generation side, transmission and distribution side, renewable energy access, distributed power supply and microgrids of future power grids. In the vigorous development of energy storage technology, the main raw material of all-vanadium liquid flow battery, electrolyte-grade ammonium metavanadate, has a bright market prospect, high product added value, and certain social and economic benefits.
[0004] At present, the domestic production methods of ammonium metavanadate mainly adopt two methods: pyrolysis roasting and wet leaching to extract vanadium. The pyrolysis roasting method is to subject the vanadium-containing materials to different roasting methods such as pyrolysis high-temperature oxidation roasting, sodium roasting, and calcium roasting, and the produced roasted sand is subjected to wet high-temperature water leaching, alkali leaching, acid leaching, etc. to obtain a vanadium-containing solution, and then add auxiliary materials to the vanadium-containing solution to obtain a vanadium product.
[0005] In terms of wet leaching vanadium extraction, Chinese invention patents disclose a variety of vanadium extraction methods, including organic extraction, direct sulfuric acid leaching of vanadium-containing raw materials, alkaline leaching, etc. The vanadium product is obtained by adding auxiliary materials to the produced vanadium-containing solution.
[0006] The technical disadvantages of the above-mentioned pyrometallurgical roasting and wet vanadium extraction methods are long process, high energy consumption, low recovery rate and high production cost. More importantly, the ammonium metavanadate product has low vanadium pentoxide content and high impurities, which cannot meet the dual demands of high-end customers for high quality and low price.
[0007] Therefore, a new technical solution is urgently needed in the prior art to solve this problem. Summary of the invention
[0008] The technical problem to be solved by the present invention is to provide a method for producing electrolyte-grade ammonium metavanadate using sodium polyvanadate as a raw material, so as to solve the technical problems that the existing method for producing ammonium metavanadate has a long process, high energy consumption, low recovery rate, high production cost, low vanadium pentoxide content, high impurities, and cannot meet the dual demands of high-end customers for high quality and low price.
[0009] A method for producing electrolyte-grade ammonium metavanadate using sodium polyvanadate as a raw material comprises the following steps, and the following steps are performed in sequence:
[0010] Step 1: weigh sodium polyvanadate and determine the contents of vanadium pentoxide V2O5 and chromium Cr in the sodium polyvanadate, mix the sodium polyvanadate and water at a solid-liquid mass ratio of 9:1, and stir to obtain a mixed slurry;
[0011] Step 2: The mixed slurry after stirring is heated to 50° C., and sodium hydroxide with a mass of 60% of the vanadium pentoxide in the sodium polyvanadate is added, and stirred for 30 minutes to dissolve it completely, thereby obtaining a leaching solution, wherein the concentration of vanadium pentoxide V2O5 in the leaching solution reaches 80 g / L to 90 g / L, and the leaching rate of the leaching solution is greater than 98.50%;
[0012] Step 3: Continue to raise the temperature to 80°C, add sodium sulfide with a chromium content of 1.05 times to the leaching solution to remove impurities, and react at a constant temperature for 40 minutes;
[0013] Step 4: Add 20% aluminum sulfate and 10% magnesium sulfate of the mass of vanadium pentoxide in the ammonium polyvanadate, stir for 5 minutes to fully dissolve, add sulfuric acid to adjust the pH value to 8-9, maintain the temperature at 80°C, react for 20 minutes to remove trace metal cation impurities in the slurry, and then pump the mixed solution into a sedimentation tank for sedimentation;
[0014] Step 5: After settling for 48 hours, the pure vanadium-containing solution is filtered through a filtering device, and the impurities are removed and bagged for subsequent recycling;
[0015] Step 6: The V2O5 concentration of the pure vanadium-containing solution is tested, and a vanadium precipitation agent is added at 1.5 times the amount of vanadium pentoxide metal to precipitate vanadium. After reacting at room temperature for 1 hour, the V2O5 concentration in the vanadium precipitation supernatant is tested. If the concentration value is less than 2g / L, it is qualified, and if the concentration value is greater than or equal to 2g / L, it is unqualified. In this case, the vanadium precipitation time needs to be extended until the vanadium precipitation supernatant passes the test, and then the vacuum suction filter tank is used for liquid-solid separation. The obtained solid is the ammonium metavanadate product. The ammonium metavanadate product is washed with pure water five times, and the ammonium metavanadate filtrate and washing water separated from the liquid-solid separation enter the filtrate pit, and the wastewater is treated after the vanadium is recovered by vanadium ion exchange.
[0016] In step 6, the vanadium precipitating agent is ammonium sulfate.
[0017] Through the above design scheme, the present invention can bring the following beneficial effects:
[0018] 1. The present invention proposes a method for producing electrolyte-grade ammonium metavanadate using sodium polyvanadate as a raw material, which uses sodium hydroxide for leaching, has a mild leaching temperature of 50°C, takes only 30 minutes to react, has low energy consumption, high production efficiency, and a leaching rate of more than 98.5%, and can directly proceed to the next process without filtering;
[0019] 2. In the impurity removal process, different impurity removers are added in sequence to achieve the purpose of thorough impurity removal at one time. The operation is simple and easy. The content of vanadium pentoxide in the produced ammonium metavanadate product after calcination is greater than 99.80%, and the impurity elements can meet the requirements of electrolyte-grade ammonium metavanadate products.
[0020] 3. The production process is short, the energy consumption is low, the recovery rate is as high as 98%, and the technical operation parameters of each process are easy to control and easy to operate.
[0021] In summary, the method for producing electrolyte-grade ammonium metavanadate using sodium polyvanadate as a raw material proposed by the present invention has a short process flow, a simple preparation method, easy operation, mild reaction conditions, low equipment requirements, low cost, and good social and economic benefits. DETAILED DESCRIPTION
[0022] In order to more clearly illustrate the purpose, technical solutions and outstanding advantages of the present invention, the present invention is further described below in conjunction with specific embodiments. The described contents are illustrative rather than restrictive and should not be used to limit the protection scope of the present invention. Matters not described in the present invention are applicable to the prior art.
[0023] Three portions of sodium polyvanadate produced by vanadium pentoxide production enterprises were selected for the following test.
[0024] Example 1
[0025] Detection and analysis data of main components of ammonium polyvanadate raw materials: (unit %)
[0026] <![CDATA[V2O5]]> From Al P Cr Fe And 75.62 1.25 1.07 0.23 0.58 6.77 7.31
[0027] Step 1: Take 500 g of sodium polyvanadate, mix the sodium polyvanadate and water at a solid-liquid ratio of 9:1, and stir to form a slurry;
[0028] Step 2: Heat the mixed slurry to 50°C, add sodium hydroxide with a mass percentage of 60% of the vanadium pentoxide in the sodium polyvanadate, stir for 30 minutes to dissolve it completely, take a small amount of dissolved slurry and filter it, the concentration of vanadium pentoxide in the test liquid is 82.98g / l, and the leaching rate is >98.50%;
[0029] Step 3: Continue to heat the sodium polyvanadate alkali leaching slurry in step 2 to 80° C., add sodium sulfide 1.05 times the mass of chromium, and react at a constant temperature for 40 minutes;
[0030] Step 4: After the sodium sulfide is added and the reaction is finished, 20% of aluminum sulfate and 10% of magnesium sulfate by mass of vanadium pentoxide in the ammonium polyvanadate are added, and after stirring for 5 minutes to fully dissolve, sulfuric acid is added to adjust the pH value to 8-9 and the temperature to 80°C. After reacting for 20 minutes, the mixed solution is pumped into a sedimentation tank for sedimentation;
[0031] Step 5: After the impurity-removed mixed liquid is settled in the sedimentation tank for 48 hours, it is filtered through the filtration equipment to obtain a pure vanadium-containing solution, and the impurity-removed residue is bagged for subsequent recycling and treatment.
[0032] Step 6: The V2O5 concentration of the pure vanadium-containing solution is tested, and a vanadium precipitator is added according to 1.5 times the amount of vanadium pentoxide metal to precipitate vanadium. After reacting at room temperature for 1 hour, the V2O5 concentration of the vanadium precipitation supernatant is tested to be 1.20g / l, and <2g / l is qualified, and then the liquid-solid separation is carried out in a vacuum suction filter tank, and the ammonium metavanadate product is washed with pure water five times. The ammonium metavanadate filtrate and the washing water enter the filtrate pit, and after the vanadium is recovered by vanadium ion exchange, the wastewater treatment is carried out and discharged after passing the wastewater treatment.
[0033] Step 7: Package the product ammonium metavanadate.
[0034] The ammonium metavanadate prepared by this method is calcined to obtain vanadium pentoxide. The component test data are as follows: (unit: %, ND means not detected)
[0035] <![CDATA[V2O5]]> From Al Yes K S P Fe Cr And 99.86 0.0082 0.0068 ND 0.0015 0.0071 0.0018 0.0033 0.0045 0.007 .
[0036] Example 2
[0037] Detection and analysis data of main components of ammonium polyvanadate raw materials: (unit %)
[0038] <![CDATA[V2O5]]> From Al P Cr Fe And 76.25 1.83 0.95 0.34 0.74 8.91 6.78
[0039] Step 1: Take 500 g of sodium polyvanadate, mix the sodium polyvanadate and water at a solid-liquid ratio of 9:1, and stir to form a slurry;
[0040] Step 2: Heat the mixed slurry to 50°C, add sodium hydroxide with a mass percentage of 60% of the vanadium pentoxide in the sodium polyvanadate, stir for 30 minutes to dissolve it completely, take a small amount of dissolved slurry and filter it, the concentration of vanadium pentoxide in the test liquid is 84.35g / l, and the leaching rate is >98.50%;
[0041] Step 3: Continue heating the sodium polyvanadate alkali leaching slurry in step 2 to 80° C., add sodium sulfide with a mass of 1 times the mass of chromium, and react at a constant temperature for 40 minutes;
[0042] Step 4: After the sodium sulfide is added and the reaction is finished, 20% of aluminum sulfate and 10% of magnesium sulfate by mass of vanadium pentoxide in the ammonium polyvanadate are added, and after stirring for 5 minutes to fully dissolve, sulfuric acid is added to adjust the pH value to 8-9 and the temperature to 80°C. After reacting for 20 minutes, the mixed solution is pumped into a sedimentation tank for sedimentation;
[0043] Step 5: After the impurity-removed mixed liquid is settled in the sedimentation tank for 48 hours, it is filtered through the filtration equipment to obtain a pure vanadium-containing solution, and the impurity-removed residue is bagged for subsequent recycling and treatment.
[0044] Step 6: The V2O5 concentration of the pure vanadium-containing solution is tested, and a vanadium precipitator is added at 1.4 times the amount of vanadium pentoxide metal to precipitate vanadium. After reacting at room temperature for 1 hour, the V2O5 concentration of the vanadium precipitation supernatant is tested to be 1.52g / l. If it is less than 2g / l, it is passed through a vacuum suction filter tank for liquid-solid separation, and the ammonium metavanadate product is washed with pure water five times. The ammonium metavanadate filtrate and the washing water enter the filtrate pit, and after the vanadium is recovered by vanadium ion exchange, the wastewater treatment is passed and discharged.
[0045] Step 7: Package the product ammonium metavanadate.
[0046] The ammonium metavanadate prepared by this method is calcined to obtain vanadium pentoxide. The component test data are as follows: (unit: %, ND means not detected)
[0047] <![CDATA[V2O5]]> From Al Yes K S P Fe Cr And 99.81 0.0068 0.0071 ND 0.0009 0.0083 0.0012 0.0025 0.0046 0.0069 .
[0048] Example 3
[0049] Detection and analysis data of main components of ammonium polyvanadate raw materials: (unit %)
[0050] <![CDATA[V2O5]]> From Al P Cr Fe And 73.21 2.23 1.39 0.28 0.87 12.96 7.17
[0051] Step 1: Take 500 g of sodium polyvanadate, mix the sodium polyvanadate and water at a solid-liquid ratio of 9:1, and stir to form a slurry;
[0052] Step 2: Heat the mixed slurry to 50°C, add sodium hydroxide with a mass percentage of 65% of the vanadium pentoxide in the sodium polyvanadate, stir for 30 minutes to dissolve it completely, take a small amount of dissolved slurry and filter it, the concentration of vanadium pentoxide in the test liquid is 80.12g / l, and the leaching rate is >98.50%;
[0053] Step 3: Continue to heat the sodium polyvanadate alkali leaching slurry in step 2 to 80° C., add sodium sulfide 1.05 times the mass of chromium, and react at a constant temperature for 40 minutes;
[0054] Step 4: After the sodium sulfide is added and the reaction is finished, 20% of aluminum sulfate and 10% of magnesium sulfate by mass of vanadium pentoxide in the ammonium polyvanadate are added, and after stirring for 5 minutes to fully dissolve, sulfuric acid is added to adjust the pH value to 8-9 and the temperature to 80°C. After reacting for 20 minutes, the mixed solution is pumped into a sedimentation tank for sedimentation;
[0055] Step 5: After the impurity-removed mixed liquid is settled in the sedimentation tank for 48 hours, it is filtered through the filtration equipment to obtain a pure vanadium-containing solution, and the impurity-removed residue is bagged for subsequent recycling and treatment.
[0056] Step 6: The V2O5 concentration of the pure vanadium-containing solution is tested, and a vanadium precipitator is added at 1.3 times the amount of vanadium pentoxide metal to precipitate vanadium. After reacting at room temperature for 1 hour, the V2O5 concentration of the vanadium precipitation supernatant is tested to be 1.87g / l. If it is less than 2g / l, it is passed through a vacuum suction filter tank for liquid-solid separation, and the ammonium metavanadate product is washed with pure water five times. The ammonium metavanadate filtrate and the washing water enter the filtrate pit, and after the vanadium is recovered by vanadium ion exchange, the wastewater treatment is passed and discharged.
[0057] Step 7: Package the product ammonium metavanadate.
[0058] The ammonium metavanadate prepared by this method is calcined to obtain vanadium pentoxide. The component test data are as follows: (unit: %, ND means not detected)
[0059] <![CDATA[V2O5]]> From Al Yes K S P Fe Cr And 99.91 0.0070 0.0045 ND 0.0009 0.0086 0.0012 0.0028 0.0022 0.0087 .
[0060] In summary, the method of the present invention comprises mixing sodium polyvanadate and water in proportion, heating the mixture to 50°C, adding sodium hydroxide which accounts for 60% of the mass of vanadium pentoxide in the sodium polyvanadate for leaching, adding three different impurity removers to the leached mixed solution respectively, and thoroughly removing impurities at one time. After the impurities are removed, the mixed solution is filtered to obtain a pure vanadium-containing solution, and a vanadium precipitation agent is added to the pure vanadium-containing solution at room temperature to precipitate vanadium to obtain the product ammonium metavanadate, and then washing with pure water five times. After calcination, the purity of the vanadium pentoxide is as high as 99.91%, and the direct yield of vanadium pentoxide is greater than 98%.
Claims
1. A method for producing electrolyte-grade ammonium metavanadate using sodium polyvanadate as a raw material, characterized in that: The process includes the following steps, which are performed in sequence: Step 1: weigh sodium polyvanadate and determine the contents of vanadium pentoxide V2O5 and chromium Cr in the sodium polyvanadate, mix the sodium polyvanadate and water at a solid-liquid mass ratio of 9:1, and stir to obtain a mixed slurry; Step 2: The mixed slurry after stirring is heated to 50° C., and sodium hydroxide with a mass of 60% of the vanadium pentoxide in the sodium polyvanadate is added, and stirred for 30 minutes to dissolve it completely, thereby obtaining a leaching solution, wherein the concentration of vanadium pentoxide V2O5 in the leaching solution reaches 80 g / L to 90 g / L, and the leaching rate of the leaching solution is greater than 98.50%; Step 3: Continue to raise the temperature to 80°C, add sodium sulfide with a chromium content of 1.05 times to the leaching solution to remove impurities, and react at a constant temperature for 40 minutes; Step 4: Add 20% aluminum sulfate and 10% magnesium sulfate of the mass of vanadium pentoxide in the ammonium polyvanadate, stir for 5 minutes to fully dissolve, add sulfuric acid to adjust the pH value to 8-9, maintain the temperature at 80°C, react for 20 minutes to remove trace metal cation impurities in the slurry, and then pump the mixed solution into a sedimentation tank for sedimentation; Step 5: After settling for 48 hours, the pure vanadium-containing solution is filtered through a filtering device, and the impurities are removed and bagged for subsequent recycling; Step 6: The V2O5 concentration of the pure vanadium-containing solution is tested, and a vanadium precipitation agent is added at 1.5 times the amount of vanadium pentoxide metal to precipitate vanadium. After reacting at room temperature for 1 hour, the V2O5 concentration in the vanadium precipitation supernatant is tested. If the concentration value is less than 2g / L, it is qualified, and if the concentration value is greater than or equal to 2g / L, it is unqualified. In this case, the vanadium precipitation time needs to be extended until the vanadium precipitation supernatant passes the test, and then the vacuum suction filter tank is used for liquid-solid separation. The obtained solid is the ammonium metavanadate product. The ammonium metavanadate product is washed with pure water five times, and the ammonium metavanadate filtrate and washing water separated from the liquid-solid separation enter the filtrate pit, and the wastewater is treated after the vanadium is recovered by vanadium ion exchange.
2. A method for producing electrolyte-grade ammonium metavanadate using sodium polyvanadate as a raw material according to claim 1, characterized in that: In step 6, the vanadium precipitating agent is ammonium sulfate.