Water-based environment-friendly two-component ceramic tile adhesive and preparation method thereof

By adopting a water-based environmentally friendly two-component ceramic tile adhesive, using a combination of acrylic emulsion and silicone modified polyurethane emulsion, combined with silicate cement and quartz sand powder, the bonding force and water resistance in the prior art are solved. and the problem of insufficient heat resistance, high-performance tile bonding effect is achieved.

CN118993639AActive Publication Date: 2024-11-22QINGYUAN LOUBANG BUILDING MATERIALS TECH CO LTD

Patent Information

Application Number
CN202410940342.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-22
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

Existing ceramic tile adhesives have shortcomings in terms of adhesion, water resistance and heat resistance. In particular, single polymer emulsions generally have defects of insufficient adhesion, poor water resistance and heat resistance, which is difficult to meet the market's high standards. Performance binder requirements.

Method used

Use water-based environmentally friendly two-component ceramic tile adhesive, including liquid and powder, which consists of acrylic emulsion and silicone modified polyurethane emulsion, and the powder consists of silicate cement, quartz sand and white carbon black, through specific The modification reaction and emulsification process are used to prepare silicone modified polyurethane emulsion and acrylic emulsion to improve the adhesive strength, water resistance and heat resistance of the binder.

Benefits of technology

It significantly improves the adhesion, water resistance and heat resistance of ceramic tile adhesives, can effectively solve the problems of low water absorption and delamination, enhances the bonding performance to vitrified bricks, marble, granite and other materials, and reduces air Drum and brick loss phenomenon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004943879840000021
    Figure BDA0004943879840000021
  • Figure BDA0004943879840000081
    Figure BDA0004943879840000081
  • Figure FDA0004943879830000011
    Figure FDA0004943879830000011
Patent Text Reader

Abstract

The invention belongs to the technical field of polymer materials and binders, and discloses a water-based environment-friendly two-component ceramic tile binder and a preparation method thereof. The two-component ceramic tile adhesive comprises a liquid material and a powder material, the liquid material is prepared from the following components in parts by weight: 50 to 80 parts of acrylic emulsion, 20 to 30 parts of organic silicon modified polyurethane emulsion and 0 to 30 parts of water; the powder material comprises the following components in parts by weight: 50-80 parts of Portland cement, 20-30 parts of quartz sand and 2-10 parts of white carbon black. The organic silicon modified polyurethane emulsion is obtained by reacting hydroxyl-terminated polyether modified polydimethoxy siloxane with diisocyanate and then carrying out hydrophilic chain extension, neutralization and emulsification. According to the ceramic tile adhesive disclosed by the invention, the specific organic silicon modified polyurethane emulsion and the acrylic emulsion are compounded for use, so that the adhesive force, the water resistance and the heat resistance of the ceramic tile adhesive can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polymer materials and adhesives, and particularly relates to a water-based environmentally friendly two-component tile adhesive and a preparation method thereof. Background Art

[0002] Tile adhesives primarily include cementitious adhesives (a powdered mixture of hydraulic binders, aggregates, and additives), disperslon adhesives (an organic binder composed of a water-based polymer emulsion, additives, and mineral fillers), and reaction resin adhesives (a single- or multi-component mixture of synthetic resins, mineral fillers, and additives that cures via a chemical reaction). Cementitious adhesives are less expensive but suffer from poor adhesion, flexibility, and weather resistance. Reactive resin adhesives offer better adhesion and weather resistance, but are less stable and require more stringent construction conditions. Disperslon adhesives are widely used due to their stability and ease of construction.

[0003] Currently, paste-based adhesives on the market mainly use acrylic acid solution, styrene acrylic emulsion, and polyvinyl acetate emulsion as water-based polymer emulsion components. However, single polymer emulsions generally have the disadvantages of insufficient bonding strength and poor water and heat resistance. Patent CN 115260947 A discloses a tile adhesive that uses a compound of acrylic acid emulsion and water-based polyurethane emulsion as colloidal components. The coating has good bonding properties. By adding polyurethane emulsion, the problem of high water absorption of acrylic emulsion can be effectively improved. Under the premise of good flexibility, the tile adhesive is given good water resistance and improved water immersion bonding performance. However, the use of ordinary water-based polyurethane emulsion compound has limited effect on improving the water resistance and heat resistance of tile adhesive.

[0004] Therefore, developing a tile adhesive with strong bonding force, good water resistance and heat resistance has broad market prospects. Summary of the Invention

[0005] In view of the shortcomings and deficiencies of the above-mentioned prior art, the primary purpose of the present invention is to provide a water-based environmentally friendly two-component tile adhesive.

[0006] Another object of the present invention is to provide a method for preparing the above-mentioned water-based environmentally friendly two-component tile adhesive.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] A water-based environmentally friendly two-component tile adhesive, comprising a liquid material and a powder material;

[0009] The liquid material comprises the following components in parts by weight: 50-80 parts of acrylic emulsion, 20-30 parts of organosilicon-modified polyurethane emulsion, and 0-30 parts of water;

[0010] The powder comprises the following components in parts by weight: 50-80 parts of Portland cement, 20-30 parts of quartz sand, and 2-10 parts of white carbon black;

[0011] The organosilicon-modified polyurethane emulsion is prepared by the following method:

[0012] Add terminal hydroxyl polyether modified polydimethoxysiloxane, diisocyanate and organotin catalyst into a reaction kettle and stir and mix evenly, heat to 70-85°C and stir to react until the NCO group content is 0.5%-2%, then add DMPA (2,2-dihydroxymethylpropionic acid) or DMBA (2,2-dihydroxymethylbutyric acid) butanone solution and continue stirring to react until the NCO group content is less than 0.2%, after the reaction is completed, cool to below 50°C, add triethylamine acetone solution for neutralization, then add deionized water and stir to emulsify, and evaporate the organic solvent under reduced pressure to obtain a silicone modified polyurethane emulsion.

[0013] The hydroxyl-terminated polyether-modified polydimethoxysiloxane is a conventional raw material in the art, and its structural formula is shown below:

[0014]

[0015] Where A is -CH2CH2CH2(OCH2CH2) a (OCH2CH(CH3)) b OH-terminated hydroxyl polyether; n is an integer of 1 to 50, a is an integer of 1 to 20, and b is an integer of 0 to 10.

[0016] The diisocyanate is preferably hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), dicyclohexylmethane diisocyanate (HMDI), toluene diisocyanate (TDI) or diphenylmethane diisocyanate (MDI).

[0017] The molar ratio of the added hydroxyl-terminated polyether-modified polydimethoxysiloxane and diisocyanate is 1:1.5-2 (OH / NCO).

[0018] The organotin catalyst is preferably dibutyltin dilaurate.

[0019] The addition amount of DMPA or DMBA is preferably 1% to 5% of the total mass of the terminal hydroxyl polyether modified polydimethoxysiloxane and diisocyanate; the addition amount of triethylamine is 1% to 5% of the total mass of the terminal hydroxyl polyether modified polydimethoxysiloxane and diisocyanate.

[0020] The solid content of the organosilicon-modified polyurethane emulsion is 30% to 50%.

[0021] The acrylic emulsion includes pure acrylic emulsion, silicone acrylic emulsion, styrene acrylic emulsion, acetate acrylic emulsion, etc. commonly used in the market; more preferably, the acrylic emulsion is a silicone-modified acrylic emulsion prepared by the following method:

[0022] (1) adding hydroxyl-terminated polyether-modified polydimethoxysiloxane, isocyanate ethyl acrylate, and an organotin catalyst into a reaction kettle and stirring and mixing them uniformly, heating to 70-85° C. and stirring to react until the NCO group content is less than 0.1%, thereby obtaining an organosilicon-modified acrylate macromonomer;

[0023] (2) adding the organosilicon-modified acrylate macromonomer, acrylic acid monomer and acrylate monomer into the emulsifier aqueous solution and stirring to emulsify uniformly, heating to 60-80° C. under nitrogen protection, adding an initiator and keeping the temperature to react, thereby obtaining an organosilicon-modified acrylic emulsion.

[0024] The raw materials such as the hydroxyl-terminated polyether-modified polydimethoxysiloxane and the organotin catalyst used in the preparation of the acrylic emulsion are of the same source as those used in the preparation of the organosilicon-modified polyurethane emulsion, and are not described in detail here.

[0025] The molar ratio of the terminal hydroxyl polyether modified polydimethoxysiloxane to the isocyanate ethyl acrylate added in step (1) is 1:1.5-2.

[0026] The acrylic acid monomer in step (2) is (meth)acrylic acid; the acrylate monomer is one or more of methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hydroxyethyl (meth)acrylate, and hydroxypropyl (meth)acrylate.

[0027] The mass ratio of the organosilicon-modified acrylate macromonomer, acrylic acid monomer and acrylate monomer added in step (2) is 1:1-3:2-4.

[0028] The emulsifier aqueous solution in step (2) is an aqueous solution of sodium allyloxyhydroxypropane sulfonate, allyloxy nonylphenol polyoxyethylene ether ammonium sulfate, alkylphenol polyoxyethylene ether ammonium sulfate, allyloxy nonylphenol polyoxyethylene ether, and alkylphenol polyoxyethylene ether with a mass concentration of 4% to 8%.

[0029] The initiator in step (2) is ammonium persulfate or potassium persulfate, and the amount of the initiator added is 0.2% to 0.8% of the total mass of the polymerization monomers.

[0030] The solid content of the organosilicon-modified acrylic emulsion is 30% to 60%.

[0031] The preparation method of the above-mentioned water-based environmentally friendly two-component tile adhesive includes the following preparation steps:

[0032] (a) adding an acrylic emulsion and a silicone-modified polyurethane emulsion into a mixing tank and stirring to mix them uniformly, and then adding water to adjust the solid content to 30% to 50% to obtain a liquid material;

[0033] (b) Portland cement, quartz sand, and white carbon black are added to a dry powder mixer and stirred to obtain a powder.

[0034] When the water-based environmentally friendly two-component tile adhesive is used, the liquid material and the powder material are directly mixed in a mass ratio of 2 to 4:1 and then applied.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] (1) The tile adhesive of the present invention is composed of a liquid and a powder, and has two outstanding features: good adhesion and environmental friendliness, with water as the dispersion medium. It is a strong adhesive anti-stripping treatment agent and enhancer. It can prevent delamination of vitrified tiles, marble, granite, etc. with low water absorption, and can effectively solve the problem of hollowing and falling tiles.

[0037] (2) The present invention uses a specific silicone-modified polyurethane emulsion and an acrylic emulsion for compounding, which can significantly improve the bonding strength, water resistance and heat resistance of the tile adhesive.

[0038] (3) The present invention can further adopt a specific silicone-modified acrylic emulsion. Compared with the silicone-acrylic emulsion prepared by conventional short-chain organosilanes, on the one hand, the mixing compatibility of acrylic emulsion and silicone-modified polyurethane emulsion is improved, and the compounding performance is further improved; on the other hand, the introduction of long-chain silicone side chains and cross-linked structures further improves the bonding strength, water resistance and heat resistance of the tile adhesive. DETAILED DESCRIPTION

[0039] The present invention will be further described in detail below with reference to examples, but the embodiments of the present invention are not limited thereto.

[0040] Example 1

[0041] A water-based environmentally friendly two-component tile adhesive, comprising a liquid material and a powder material;

[0042] The liquid material comprises the following components in parts by weight: 60 parts of pure acrylic emulsion (commercially available, solid content 48%), 25 parts of organosilicon-modified polyurethane emulsion (solid content 42%), and 2.7 parts of water.

[0043] The powder comprises the following components in parts by weight: 70 parts of Portland cement, 25 parts of quartz sand, and 5 parts of white carbon black.

[0044] The organosilicon-modified polyurethane emulsion is prepared by the following method:

[0045] The terminal hydroxyl polyether modified polydimethoxysiloxane (the average molecular weight of the polydimethoxysiloxane segment is 2000, and the terminal hydroxyl polyether is propyl polyoxyethylene ether with an average molecular weight of 800) is dehydrated under reduced pressure, added into a reaction kettle with hexamethylene diisocyanate (HDI) and a catalytic amount of dibutyltin dilaurate, and stirred and mixed evenly. The molar ratio of the terminal hydroxyl polyether modified polydimethoxysiloxane to HDI is 1:1.8. The temperature is raised to 80°C and stirred for 2.5h. The NCO group content of the product is detected to be 1.02%. A DMPA butanone solution with a total mass of 2.4% of terminal hydroxyl polyether-modified polydimethoxysiloxane and diisocyanate was added, and the reaction was continued with stirring for 1.5 hours. The NCO group content of the product was detected to be 0.16%. After the reaction was completed, the temperature was lowered to below 50°C, and a triethylamine acetone solution with the same mass as DMPA was added for neutralization and stirring for 0.5 hours. Deionized water was then added and stirred for emulsification. The organic solvents (acetone and butanone) were evaporated under reduced pressure, and deionized water was added during the evaporation process to obtain a silicone-modified polyurethane emulsion with a solid content of 42%.

[0046] Example 2

[0047] A water-based environmentally friendly two-component tile adhesive, comprising a liquid material and a powder material;

[0048] The liquid material comprises the following components in parts by weight: 80 parts of pure acrylic emulsion (commercially available, solid content 48%), 20 parts of organosilicon-modified polyurethane emulsion (solid content 50%), and 7.6 parts of water.

[0049] The powder comprises the following components in parts by weight: 50 parts of Portland cement, 30 parts of quartz sand, and 10 parts of white carbon black.

[0050] The organosilicon-modified polyurethane emulsion is prepared by the following method:

[0051] The terminal hydroxyl polyether modified polydimethoxysiloxane (the average molecular weight of the polydimethoxysiloxane segment is 1000, and the terminal hydroxyl polyether is propyl polyoxyethylene polyoxypropylene ether with an average molecular weight of 600) is dehydrated under reduced pressure, added to the reactor with isophorone diisocyanate (IPDI) and a catalytic amount of dibutyltin dilaurate, and stirred and mixed evenly. The molar ratio of the terminal hydroxyl polyether modified polydimethoxysiloxane to IPDI is 1:1.5. The temperature is raised to 75°C and stirred for 3 hours. The NCO group content of the product is detected to be 0.85%. , then add DMPA butanone solution with a total mass of 1.8% of terminal hydroxyl polyether modified polydimethoxysiloxane and diisocyanate and continue stirring to react for 2 hours. The NCO group content of the product is detected to be 0.13%. After the reaction is completed, the temperature is lowered to below 50°C, and triethylamine acetone solution with the same mass as DMPA is added for neutralization and stirring to react for 0.5 hours. Then, deionized water is added and stirred to emulsify. The organic solvents (acetone and butanone) are evaporated under reduced pressure. Deionized water is added during the evaporation process to obtain a silicone-modified polyurethane emulsion with a solid content of 50%.

[0052] Example 3

[0053] A water-based environmentally friendly two-component tile adhesive, comprising a liquid material and a powder material;

[0054] The liquid material comprises the following components in parts by weight: 50 parts of pure acrylic emulsion (commercially available, solid content 48%), and 30 parts of organosilicon-modified polyurethane emulsion (solid content 36%).

[0055] The powder comprises the following components in parts by weight: 80 parts of Portland cement, 20 parts of quartz sand, and 2 parts of white carbon black.

[0056] The organosilicon-modified polyurethane emulsion is prepared by the following method:

[0057] The terminal hydroxyl polyether modified polydimethoxysiloxane (the average molecular weight of the polydimethoxysiloxane segment is 3000, and the terminal hydroxyl polyether is propyl polyoxyethylene ether with an average molecular weight of 1200) is dehydrated under reduced pressure, added into a reaction kettle with toluene diisocyanate (TDI) and a catalytic amount of dibutyltin dilaurate, and stirred and mixed evenly. The molar ratio of the terminal hydroxyl polyether modified polydimethoxysiloxane to TDI is 1:1.9. The temperature is raised to 85°C and stirred for 2.5 hours. The NCO group content of the product is detected to be 1.31%. Add 3.0% of the total mass of terminal hydroxyl polyether modified polydimethoxysiloxane and diisocyanate DMBA butanone solution and continue stirring to react for 2 hours. The NCO group content of the product is detected to be 0.18%. After the reaction is completed, the temperature is lowered to below 50°C, and triethylamine acetone solution with the same mass as DMBA is added for neutralization and stirring reaction for 0.5 hours. Then, deionized water is added and stirred for emulsification. The organic solvents (acetone and butanone) are evaporated under reduced pressure. Deionized water is added during the evaporation process to obtain a silicone modified polyurethane emulsion with a solid content of 36%.

[0058] Example 4

[0059] A water-based environmentally friendly two-component tile adhesive is disclosed. Compared with Example 1, silicone acrylic emulsion (commercially available, solid content 48%) is used instead of pure acrylic emulsion, and the rest of the adhesive is the same.

[0060] Example 5

[0061] A water-based environmentally friendly two-component tile adhesive is disclosed. Compared with Example 1, silicone-modified acrylic emulsion (solid content 48%) is used instead of pure acrylic emulsion, and the rest of the adhesive is the same.

[0062] The preparation method of the organosilicon-modified acrylic emulsion is as follows:

[0063] (1) Add terminal hydroxyl polyether modified polydimethoxysiloxane (the average molecular weight of the polydimethoxysiloxane segment is 2000, and the terminal hydroxyl polyether is propyl polyoxyethylene ether with an average molecular weight of 800) and ethyl isocyanate acrylate in a molar ratio of 1:1.8 and a catalytic amount of dibutyltin dilaurate into a reactor and stir to mix evenly. Heat to 80°C and stir to react for 4 hours. The NCO group content of the product is detected to be 0.09%, thereby obtaining a silicone modified acrylate macromonomer.

[0064] (2) The silicone-modified acrylate macromonomer, acrylic acid, methyl methacrylate, and butyl acrylate were added in a mass ratio of 1:1.5:1:1.5 to a 5% aqueous solution of an emulsifier (composed of allyloxy nonylphenol polyoxyethylene ether and nonylphenol polyoxyethylene ether in a mass ratio of 1:1) and stirred to emulsify evenly. The temperature was raised to 75°C under nitrogen protection, and 0.4% ammonium persulfate was added and kept warm for 4 hours to obtain a silicone-modified acrylic emulsion.

[0065] Comparative Example 1

[0066] A water-based environmentally friendly two-component tile adhesive is prepared. Compared with Example 1, a commercially available polyurethane emulsion (R8402B water-based polyurethane emulsion, solid content 42%, from Guangzhou Ruilin New Materials Co., Ltd.) is used instead of the silicone-modified polyurethane emulsion, and the rest of the steps are the same.

[0067] Comparative Example 2

[0068] A water-based environmentally friendly two-component tile adhesive is prepared. Compared with Example 5, a commercially available polyurethane emulsion (R8402B water-based polyurethane emulsion, solid content 42%, from Guangzhou Ruilin New Materials Co., Ltd.) is used instead of the silicone-modified polyurethane emulsion, and the rest of the steps are the same.

[0069] The tile adhesives of the above examples and comparative examples were tested for performance. Liquid and powder were mixed in a mass ratio of 2:1 according to JC / T 547-2017. The test results are shown in Table 1 below.

[0070] Table 1

[0071]

[0072]

[0073] As shown in Table 1, a comparison of Examples 1-4 with Comparative Example 1 demonstrates that the specific organosilicon-modified polyurethane emulsions and acrylic emulsions used in the present invention significantly improve the adhesion, water resistance, and heat resistance of the tile adhesive compared to conventional polyurethane emulsions. A comparison of Example 5 with Examples 1-4 and Comparative Example 2 demonstrates that the combination of the organosilicon-modified acrylic emulsions and organosilicon-modified polyurethane emulsions of the present invention further significantly improves the adhesion, water resistance, and heat resistance of the resulting tile adhesive compared to conventional acrylic emulsions.

[0074] The above embodiments are preferred implementations of the present invention, but the implementations of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be considered as equivalent replacement methods and are included in the scope of protection of the present invention.

Claims

1. A water-based environmentally friendly two-component tile adhesive, characterized in that: Including liquid and powder; The liquid material comprises the following components in parts by weight: 50 to 80 parts of acrylic emulsion, 20 to 30 parts of organosilicon-modified polyurethane emulsion, and 0 to 30 parts of water; The powder comprises the following components in parts by weight: 50-80 parts of Portland cement, 20-30 parts of quartz sand, and 2-10 parts of white carbon black; The organosilicon-modified polyurethane emulsion is prepared by the following method: Add terminal hydroxyl polyether modified polydimethoxysiloxane, diisocyanate and organotin catalyst into a reaction kettle and stir to mix evenly, heat to 70-85°C and stir to react until the NCO group content is 0.5%-2%, then add DMPA or DMBA butanone solution and continue to stir to react until the NCO group content is less than 0.2%, after the reaction is completed, cool to below 50°C, add triethylamine acetone solution for neutralization, then add deionized water and stir to emulsify, evaporate the organic solvent under reduced pressure to obtain organosilicon modified polyurethane emulsion.

2. The water-based environmentally friendly two-component tile adhesive according to claim 1, characterized in that: The structural formula of the hydroxy-terminated polyether-modified polydimethoxysiloxane is as follows: Where A is -CH2CH2CH2(OCH2CH2) a (OCH2CH(CH3)) b OH-terminated polyether; n is an integer of 1 to 50, a is an integer of 1 to 20, and b is an integer of 0 to 10; The diisocyanate is hexamethylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate or diphenylmethane diisocyanate; The molar ratio of the terminal hydroxyl polyether modified polydimethoxysiloxane and diisocyanate added is 1:1.5-2.

3. The water-based environmentally friendly two-component tile adhesive according to claim 1, characterized in that: The added amount of DMPA or DMBA is 1% to 5% of the total mass of the terminal hydroxyl polyether modified polydimethoxysiloxane and diisocyanate; the added amount of triethylamine is 1% to 5% of the total mass of the terminal hydroxyl polyether modified polydimethoxysiloxane and diisocyanate.

4. The water-based environmentally friendly two-component tile adhesive according to claim 1, characterized in that: The solid content of the organosilicon-modified polyurethane emulsion is 30% to 50%; the acrylic emulsion is a pure acrylic emulsion, a silicone acrylic emulsion, a styrene acrylic emulsion or a acetic acid acrylic emulsion with a solid content of 30% to 60%.

5. The water-based environmentally friendly two-component tile adhesive according to claim 1, characterized in that: The acrylic emulsion is a silicone-modified acrylic emulsion prepared by the following method: (1) adding hydroxyl-terminated polyether-modified polydimethoxysiloxane, isocyanate ethyl acrylate and an organotin catalyst into a reaction kettle and stirring and mixing them evenly, heating to 70-85° C. and stirring and reacting until the NCO group content is less than 0.1%, thereby obtaining an organosilicon-modified acrylate macromonomer; (2) adding the organosilicon-modified acrylate macromonomer, acrylic acid monomer and acrylate monomer into the emulsifier aqueous solution and stirring to emulsify uniformly, heating to 60-80° C. under nitrogen protection, adding an initiator and maintaining the temperature for reaction, thereby obtaining an organosilicon-modified acrylic emulsion.

6. The water-based environmentally friendly two-component tile adhesive according to claim 5, characterized in that: The molar ratio of the terminal hydroxyl polyether modified polydimethoxysiloxane to isocyanate ethyl acrylate added in step (1) is 1:1.5-2.

7. The water-based environmentally friendly two-component tile adhesive according to claim 5, characterized in that: The acrylic acid monomer in step (2) is (meth)acrylic acid; the acrylic acid ester monomer is one or more of methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hydroxyethyl (meth)acrylate, and hydroxypropyl (meth)acrylate.

8. The water-based environmentally friendly two-component tile adhesive according to claim 5, characterized in that: The mass ratio of the organosilicon-modified acrylate macromonomer, acrylic acid monomer and acrylate monomer added in step (2) is 1:1-3:2-4.

9. The water-based environmentally friendly two-component tile adhesive according to claim 5, characterized in that: The emulsifier aqueous solution in step (2) is an aqueous solution of sodium allyloxyhydroxypropane sulfonate, allyloxy nonylphenol polyoxyethylene ether ammonium sulfate, alkylphenol polyoxyethylene ether ammonium sulfate, allyloxy nonylphenol polyoxyethylene ether, and alkylphenol polyoxyethylene ether with a mass concentration of 4% to 8%; the initiator is ammonium persulfate or potassium persulfate, and the amount of the initiator added is 0.2% to 0.8% of the total mass of the polymerized monomers.

10. The method for preparing a water-based environmentally friendly two-component tile adhesive according to any one of claims 1 to 9, characterized in that: The method comprises the following preparation steps: (a) adding acrylic emulsion and organosilicon-modified polyurethane emulsion into a mixing tank, stirring and mixing, and then adding water to adjust the solid content to 30% to 50% to obtain a liquid material; (b) Add silicate cement, quartz sand and white carbon black into a dry powder mixer and stir to mix well to obtain powder.

Citation Information

Patent Citations

  • Organosilicon modified aqueous polyurethane emulsion

    CN103059258A

  • Preparation method for cement-based composite material used for sound barrier anchorage of high-speed railways

    CN107935514A

  • New and old pavement base splicing interface treatment material and preparation method thereof

    CN110668754A

  • Quick-drying type ceramic tile water-based adhesive as well as preparation method and equipment thereof

    CN110950614A

  • Ceramic tile back adhesive

    CN115260947A

Cited By

  • High-durability ceramic tile adhesive and preparation process thereof

    CN119954449A

  • A high-durability tile adhesive and its preparation process

    CN119954449B

  • Basalt fiber reinforced ceramic tile binder and preparation method thereof

    CN121470885A

  • A basalt fiber reinforced tile adhesive and a method of making the same

    CN121470885B