Foaming ceramic based on copper-molybdenum tailings and preparation method thereof

By using the combination of copper-molybdenum tailings and other auxiliary raw materials, dry ball milling and low-temperature sintering processes are used to solve the problems of high sintering temperature and complex process in the existing technology, and achieve low density, high compressive strength and low thermal conductivity. The preparation of foamed ceramics simplifies the process flow and improves production efficiency.

CN118993760AActive Publication Date: 2024-11-22WUHAN UNIV OF TECH +1

Patent Information

Application Number
CN202410951239.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-22
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

In the prior art, the sintering temperature is high when using copper-molybdenum tailings to prepare foamed ceramics, which consumes a lot of energy, is complex in the process and has a long production cycle, is uneven in the pore size and weak pore walls, making it difficult to achieve industrial application.

Method used

Using raw materials such as copper-molybdenum tailings, potassium feldspar, sodium carbonate, waste glass, dolomite and silicon carbide, through dry ball milling and low-temperature sintering technology, combined with calcium phosphate as a foam stabilizer, the sintering temperature is reduced to 940-990℃, forming Foamed ceramics with low density, high compressive strength and low thermal conductivity.

Benefits of technology

It has achieved high dosage of copper molybdenum tailings, reduced firing energy consumption, simplified process flow, improved production efficiency, and prepared foamed ceramics with uniform pore size, high compressive strength and low thermal conductivity, with good economical and Social benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947298490000041
    Figure BDA0004947298490000041
  • Figure BDA0004947298490000051
    Figure BDA0004947298490000051
  • Figure BDA0004947298490000052
    Figure BDA0004947298490000052
Patent Text Reader

Abstract

The invention discloses foamed ceramic based on copper-molybdenum tailings and a preparation method of the foamed ceramic, and the foamed ceramic comprises the following raw materials in parts by weight: 55-80 parts of copper-molybdenum tailings, 5-20 parts of potassium feldspar, 25 parts of a fluxing agent, 0.5-1.5 parts of a foaming agent and 1-3 parts of a foam stabilizer. Wherein the fluxing agent is composed of sodium carbonate and waste glass, and the sodium carbonate accounts for 12-32% by mass of the fluxing agent; the foaming agent is composed of dolomite and silicon carbide; the foam stabilizer is calcium phosphate. The preparation method comprises the following steps: ball-milling and mixing the raw materials by a dry method, uniformly paving the mixture in a mold, and finally sintering at 940-990 DEG C to prepare the ceramic. The obtained foamed ceramic is small in density, high in compressive strength and low in heat conductivity coefficient, the sintering temperature is reduced to 940-990 DEG C while high-doping-amount utilization of the copper-molybdenum tailings is achieved, energy consumption in the sintering process is reduced, and good economic benefits and social benefits are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of foamed ceramics for construction, and in particular relates to a foamed ceramic based on copper-molybdenum tailings and a preparation method thereof. Background Art

[0002] Copper-molybdenum tailings are industrial wastes generated during the mining and selection of copper-molybdenum ores, and generally contain a wide variety of heavy metal elements. Copper-molybdenum tailings have a high annual output, a large total stockpile volume, and a low comprehensive utilization rate, which can easily cause pollution and damage to the environment and ecology.

[0003] Foamed ceramic material is a new type of building material developed in recent years, with the advantages of light weight, high hardness and low thermal conductivity. After proper treatment, copper-molybdenum tailings can be used as high-quality raw materials for firing foamed ceramics. Using copper-molybdenum tailings to fire foamed ceramics is an effective way to convert industrial waste into high value-added products.

[0004] Chinese invention patent CN104926283 A (A kind of building ceramics prepared by using copper-molybdenum tailings and its preparation method) discloses a kind of building ceramics prepared by using copper-molybdenum tailings and its preparation method, which adopts wet ball milling and pressing molding process. The preparation process is relatively complicated. The firing temperature of ceramic floor tiles is 1160±10℃, and the firing temperature of ceramic interior wall tiles is 1080±10℃. The firing temperatures of both ceramic materials are significantly higher than 1000℃.

[0005] Chinese invention patent CN103936454 A (A porous thermal insulation ceramic with gold-copper tailings as main raw materials and a preparation method thereof) introduces a porous thermal insulation ceramic with gold-copper tailings as main raw materials and a preparation method thereof, with a sintering temperature of 1000-1100°C, a large amount of silicon carbide in the foaming agent, a long ball milling time, and mold pressing. The obtained foamed ceramic has poor pore roundness and the pore size is too large.

[0006] Chinese invention patent CN107500800 B (porous ceramic material containing copper tailings and preparation method thereof) discloses a porous ceramic material containing copper tailings and a preparation method thereof, but the sintering temperature is between 1140 and 1180°C, which is relatively high, and repeated acid leaching treatment is required, so the preparation process is relatively complicated.

[0007] Chinese invention patent CN105541296 A (A method for preparing ceramic materials using copper tailings) discloses a method for preparing ceramic materials using copper tailings, wherein the amount of copper tailings used is only 35 to 55 parts, the firing temperature is 1080 to 1160°C, the firing temperature is also relatively high, and wet ball milling and pressing or extrusion molding processes are also used.

[0008] In summary, in the prior art, when using copper-containing tailings to prepare foamed ceramics, the sintering temperature is relatively high, mostly at 1000-1180°C, the firing cycle is relatively long, and a large amount of electrical and thermal energy is consumed. At the same time, the preparation process is relatively complex, and many control parameters are required. Currently, wet ball milling is mostly used, which takes a long time and consumes high energy. It requires a combination of multiple process methods such as molding and spray drying, resulting in a long production cycle and high production energy consumption. Summary of the invention

[0009] In view of the deficiencies in the above-mentioned prior art, the present invention provides a foamed ceramic based on copper-molybdenum tailings and a preparation method thereof. The foamed ceramic has uniform pore size and high roundness, low density, high compressive strength, low thermal conductivity, and a large amount of copper-molybdenum tailings. The sintering temperature during preparation is low, the process is simple, and it is conducive to industrial application.

[0010] In order to achieve the above object, the present invention adopts the following technical solutions:

[0011] The present invention provides a foamed ceramic based on copper-molybdenum tailings. The raw materials include the following components by weight: 55-80 parts of copper-molybdenum tailings, 5-20 parts of potassium feldspar, 25 parts of flux, 0.5-1.5 parts of foaming agent and 1-3 parts of foam stabilizer; wherein:

[0012] The flux is composed of sodium carbonate and waste glass, and the mass percentage of sodium carbonate in the flux is 12-32%; the foaming agent is composed of dolomite and silicon carbide; and the foam stabilizer is calcium phosphate.

[0013] According to the above scheme, the main chemical components of the copper-molybdenum tailings are SiO2 66-71wt%, Al2O3 15-20wt%, CaO 0.5-3.0wt%, MgO 0.5-3.0wt%, K2O 2-4wt%, Na2O 2-4wt%, Fe2O3 0.2-1.8wt%, CuO 0.06-0.15wt%, and MoO3 0.01-0.15wt%.

[0014] According to the above scheme, the mass percentage of sodium carbonate in the flux is 15-25%.

[0015] According to the above scheme, in the foaming agent, the mass ratio of dolomite to silicon carbide is 4:1 to 5:1.

[0016] According to the above scheme, the density of the foamed ceramic based on copper-molybdenum tailings is 400-850 kg / m 3 ; The compressive strength is 4.77~19.25MPa; The thermal conductivity is less than 0.15W / (m·K).

[0017] According to the above scheme, the sintering temperature of the copper-molybdenum tailings-based foamed ceramic is 940-990°C.

[0018] According to the above scheme, the raw materials are dry-milled and mixed, then evenly spread into a mold, and finally sintered at a temperature of 940 to 990°C to obtain the obtained product.

[0019] Provided is a method for preparing a foamed ceramic based on copper-molybdenum tailings, comprising the following steps:

[0020] 1) Ball milling and mixing: dry-milling and mixing the dried copper-molybdenum tailings, potassium feldspar and waste glass respectively; then, mixing the copper-molybdenum tailings, potassium feldspar and waste glass after ball milling with sodium carbonate, foaming agent and foam stabilizer, and then dry-milling and mixing, passing through a 200-mesh sieve, and drying to obtain a mixed powder;

[0021] 2) Evenly spreading the material: evenly spread the dry mixed powder obtained in step 1) into the mold, vibrate it, and scrape the surface of the mixed material flat;

[0022] 3) Low-temperature firing: sintering the mold filled with the mixed powder obtained in step 2) at a temperature of 940-990° C., and cooling to obtain the copper-molybdenum tailings-based foamed ceramics.

[0023] According to the above scheme, in step 1), the drying conditions are: rapid drying at 130-150° C. for 1-3 hours.

[0024] According to the above scheme, in step 1), the copper-molybdenum tailings, potassium feldspar and waste glass are dry-milled for 0.5 to 1 hour; then the ball-milled copper-molybdenum tailings, potassium feldspar and waste glass are shaken and mixed with sodium carbonate, foaming agent and foam stabilizer, and then dry-milled for 1 to 2 hours.

[0025] According to the above scheme, in the step 1), the sieving is through a 200-mesh sieve.

[0026] According to the above scheme, in step 3), the sintering time is 15 to 25 minutes.

[0027] According to the above scheme, in step 3), the sintering temperature is 950-980°C.

[0028] According to the above scheme, the heating program in step 3) is: room temperature-730°C, heating rate is 8-12°C / min; 730°C-900°C, heating rate is 8-10°C / min; keeping at 900°C for 5-10min; 900°C-sintering temperature, heating rate is 3-4°C / min.

[0029] The present invention provides a low-temperature fired copper-molybdenum tailings foamed ceramic, which is obtained by using copper-molybdenum tailings and potassium feldspar as main raw materials, sodium carbonate and waste glass as flux, dolomite and silicon carbide as foaming agents, and calcium phosphate as a foam stabilizer, wherein:

[0030] By mixing and fluxing waste glass and sodium carbonate in appropriate proportions, on the one hand, the waste glass has a low melting temperature and begins to vitrify at about 730°C. After the waste glass is melted, the liquid phase ratio and fluidity of the mixture at high temperature can be increased, and the gas generated by the foaming agent at high temperature can be better covered, and pores can be formed after cooling; while sodium carbonate produces more free Na2O when it is melted at high temperature. Na2O and K2O in the mixture can destroy the network structure of [SiO4] tetrahedron in the raw material at high temperature, effectively reducing the eutectic point of the mixed powder, so that the sintering temperature of the foamed ceramic can be reduced to below 1000°C. At the same time, the present invention introduces calcium phosphate as a foam stabilizer, which can fill the gaps between pores and serve as a component of the foamed ceramic skeleton. On the other hand, the calcium element helps to form the calcium feldspar crystal phase during cooling, avoiding excessive bubble formation caused by the strong fluxing effect of waste glass and sodium carbonate, playing a foam stabilizing role, and improving the compressive strength of the foamed ceramic. At the same time, phosphorus can participate in the formation of the glass network structure, and iron can enter the phosphate glass network structure during firing, thereby reducing the adverse coloring effect of impure iron elements in the mixed powder.

[0031] In addition, dolomite and silicon carbide are used as mixed foaming agents. SiC is oxidized at high temperature to produce gas. After the mixed powder is melted at high temperature, it is wrapped in the melt and cooled to form a closed-cell foamed ceramic. The main component of dolomite is calcium magnesium carbonate, which slowly decomposes at 730-910°C to produce carbon dioxide gas, and at the same time provides free CaO and MgO for the mixed powder, which plays a certain role in fluxing. If dolomite is used alone as a foaming agent, the amount of foaming agent will be greatly increased, which may cause the CaO content in the mixed powder to be too high, resulting in rapid deterioration of the pores of the foamed ceramic, and it is difficult to form uniform pores. At the same time, because the sintering temperature range is 940-990°C, the gas produced by the premature decomposition of dolomite is likely to escape in large quantities, resulting in poor foaming effect. Therefore, dolomite and silicon carbide are used as mixed foaming agents. The two assist in foaming, ensuring that sufficient gas is generated while playing a certain role in fluxing.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] 1. The present invention provides a low-temperature fired copper-molybdenum tailings foamed ceramic, which is obtained by using copper-molybdenum tailings and potassium feldspar as main raw materials, sodium carbonate and waste glass as fluxing agents, dolomite and silicon carbide as foaming agents, and calcium phosphate as a foam stabilizer; wherein: waste glass and sodium carbonate are mixed to assist in fluxing, which can effectively reduce the sintering temperature of the mixed powder, while waste glass, as a low-melting-point raw material, melts at high temperature to form a liquid phase, which better covers the gas generated by the foaming agent at high temperature, and potassium feldspar is used to adjust the viscosity of the mixed powder at high temperature, thereby broadening the melting range of the mixed powder. The foaming agent generates gas at high temperature, which is wrapped by the molten liquid phase and forms pores after cooling. The foam stabilizer calcium phosphate in the component can prevent the mixed powder from having more bubbles after melting, which would seriously deteriorate the pore size of the foamed ceramic. Through the coordinated use of flux, foaming agent and foam stabilizer, the sintering temperature is reduced to 940-990℃ while realizing the high-dosage utilization of copper-molybdenum tailings, which reduces the energy consumption during the firing process and prepares copper-molybdenum tailings foamed ceramics with low density, high compressive strength and low thermal conductivity, which has good economic and social benefits.

[0034] 2. The present invention provides a method for preparing low-temperature fired copper-molybdenum tailings foamed ceramics. The dry ball milling process is adopted to directly and evenly spread the obtained mixed powder in a mold for firing, thereby eliminating the pressing and molding step. This not only optimizes the production process of the foamed ceramics, but also improves the production efficiency, providing a simpler and more effective way for the large-scale manufacture of foamed ceramics. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a stereomicroscope image (1.5 times magnified) of the copper-molybdenum tailings foamed ceramic in Example 6 of the present invention. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The chemical composition of the copper-molybdenum tailings used in the embodiment is measured by X-ray fluorescence spectrometer, and includes, by weight percentage, SiO2 68.61wt%, Al2O3 17.42wt%, CaO 0.96wt%, MgO 0.94wt%, Fe2O3 1.30wt%, SO31.07wt%, K2O 3.36wt%, Na2O 3.63wt%, CuO 0.13wt%, MoO3 0.01wt%, loss on ignition is 1.81wt%, and it also contains a small amount of rare earth elements.

[0038] In the embodiments and comparative examples, the flux is composed of sodium carbonate and waste glass; the foaming agent is composed of dolomite and silicon carbide, wherein the mass ratio of dolomite to silicon carbide is 4:1; and the foam stabilizer is calcium phosphate.

[0039] The standard range of density, compressive strength and thermal conductivity in the performance indicators of foamed ceramic partition materials (T / CBCSA12-2019) is used as the screening criteria for qualified products, as shown in Table 1.

[0040] Table 1 Performance indicators of foamed ceramic partition materials (T / CBCSA12-2019)

[0041]

[0042]

[0043] Example 1

[0044] Provided is a method for preparing low-temperature fired copper-molybdenum tailings foamed ceramics, comprising the following steps:

[0045] The dried copper-molybdenum tailings, potassium feldspar, and waste glass were dry-milled for 0.5 hours respectively. According to the weight, 70 parts of copper-molybdenum tailings, 5 parts of potassium feldspar, 25 parts of flux (including 21 parts of waste glass and 4 parts of sodium carbonate), 1 part of foaming agent (the mass ratio of dolomite to silicon carbide is 4:1) and 2 parts of foam stabilizer were weighed, all the materials were shaken and mixed, and then dry-milled for 1.5 hours, passed through a 200-mesh sieve, and the part under the sieve was quickly dried at 150°C for 2 hours, and then the dried mixed powder was evenly spread into the mold, vibrated, and the surface of the mixed powder was scraped flat. The mold containing the mixed powder is fired, and the heating program is: room temperature to 730°C, the heating rate is 10°C / min; 730°C to 900°C, the heating rate is 8°C / min; keep warm at 900°C for 5min; 900°C to 960°C, the heating rate is 4°C / min; keep warm at 960°C for 20min, and process and cut after cooling in the furnace to obtain copper-molybdenum tailings foamed ceramics. The raw material composition and properties of this embodiment are shown in Table 2.

[0046] Example 2

[0047] The preparation steps are the same as those in Example 1. The detailed raw material composition and properties are shown in Table 2.

[0048] Comparative Example 1

[0049] The preparation steps are the same as those in Example 1. The detailed raw material composition and properties are shown in Table 2.

[0050] Table 2. Raw material composition and properties of Examples 1 to 2 and Comparative Example 1

[0051]

[0052] Table 2 shows that when the amount of sodium carbonate added is too small, such as in Comparative Example 1, the density of the obtained copper-molybdenum tailings foamed ceramic is too large, greater than 1g / cm 3 This is because the amount of sodium carbonate added is too little, resulting in insufficient melting and foaming of the mixed powder. As the amount of sodium carbonate added increases, the density of the resulting ceramic gradually decreases. However, when the amount of sodium carbonate added is too high, it will cause the mixed powder to melt excessively and foam, forming large pores with a pore size of more than 3mm. The pore walls are thinner and the support between the pore walls is weak, thereby reducing the compressive strength. Even if there is a foam stabilizer, its role is still limited. Therefore, the waste glass and sodium carbonate in the flux, at a suitable ratio, can reduce the sintering temperature while ensuring a balance between density, compressive strength and thermal conductivity.

[0053] Example 3

[0054] Provided is a method for preparing low-temperature fired copper-molybdenum tailings foamed ceramics, comprising the following steps:

[0055] The dried copper-molybdenum tailings, potassium feldspar, and waste glass were dry-milled for 0.5 hours respectively. According to the weight, 70 parts of copper-molybdenum tailings, 5 parts of potassium feldspar, 25 parts of flux (including 20 parts of waste glass and 5 parts of sodium carbonate), 1.0 part of foaming agent (the mass ratio of dolomite and silicon carbide is 4:1), and 1.0 part of foam stabilizer were weighed, all the materials were shaken and mixed, and then dry-milled for 1 hour, passed through a 200-mesh sieve, and the part under the sieve was taken and placed at 150°C for rapid drying for 2 hours, and then the dried mixed powder was evenly spread into the mold, vibrated, and the surface of the mixed powder was scraped flat. The mold filled with the mixed powder is sintered according to the heating program. The specific heating program is: room temperature-730℃, heating rate is 10℃ / min; 730℃-900℃, heating rate is 9℃ / min; keeping at 900℃ for 10min; 900℃-960℃, heating rate is 4℃ / min; keeping at 960℃ for 20min, cooling with the furnace and then processing and cutting to obtain copper-molybdenum tailings foamed ceramics.

[0056] Embodiment 4-5

[0057] The preparation steps are the same as those of Example 3, wherein the raw material compositions of Example 4 and Example 5 contain 1.0 part and 1.5 parts of the foaming agent respectively. The raw material composition and properties are shown in Table 3.

[0058] Table 3. Raw material composition and properties of Examples 3 to 5

[0059]

[0060] Table 3 shows that as the amount of foaming agent added in Example 3, Example 4, and Example 5 gradually increases, the apparent density of the prepared foamed ceramic samples decreases accordingly, the compressive strength also decreases, and the thermal conductivity increases. This is because, when the amount of foaming agent increases, the gas generated in the foaming process increases, the pores grow larger, resulting in a larger pore size of the foamed ceramic, a larger sample volume expansion, and thus a smaller sample density; at the same time, due to the growth and aggregation of bubbles, the average pore size increases while the pore walls become thinner, and the supporting effect between the pore walls is weakened, resulting in a smaller compressive strength of the sample and an increase in the thermal conductivity.

[0061] Example 6

[0062] Provided is a method for preparing low-temperature fired copper-molybdenum tailings foamed ceramics, comprising the following steps:

[0063] The dried copper-molybdenum tailings, potassium feldspar, and waste glass were dry-milled for 1 hour respectively. According to the weight, 55 parts of copper-molybdenum tailings, 20 parts of potassium feldspar, 25 parts of flux (including 20 parts of waste glass and 5 parts of sodium carbonate), 1.0 parts of foaming agent (the mass ratio of dolomite and silicon carbide is 4:1), and 1.5 parts of foam stabilizer were weighed. All materials were shaken and mixed and dry-milled for 1.5 hours. After the ball milling was completed, the mixture was sieved through a 200-mesh sieve, and the part under the sieve was taken and placed under 150°C for rapid drying for 2 hours to obtain a dry mixed powder for use. The dry mixed powder was evenly spread into the mold, vibrated, and the surface of the mixed powder was scraped flat.

[0064] The mold filled with the mixed powder is fired according to the heating program. The specific heating program is: room temperature-730℃, heating rate is 10℃ / min; 730℃-900℃, heating rate is 9℃ / min; keeping at 900℃ for 10min; 900℃-960℃, heating rate is 4℃ / min; keeping at sintering temperature of 960℃ for 20min, cooling with the furnace and then processing and cutting to obtain copper-molybdenum tailings foamed ceramics.

[0065] Figure 1 This is a stereomicroscope image of the copper-molybdenum tailings foamed ceramic prepared in this example, which shows that the pores of the foamed ceramic have a high degree of roundness, uniform pore size, and moderate pore wall thickness.

[0066] Embodiment 7-8

[0067] The preparation steps of Example 7 and Example 8 are the same as those of Example 6. The detailed raw material compositions and properties are shown in Table 4.

[0068] Table 4. Raw material composition and properties of Examples 6 to 8

[0069]

[0070] Table 4 shows that Example 6, Example 7, and Example 8 all meet the performance indicators of density numbers 500, 600, and 800, respectively, and the prepared foamed ceramics have good performance.

[0071] Example 9

[0072] Provided is a method for preparing low-temperature fired copper-molybdenum tailings foamed ceramics, comprising the following steps:

[0073] The dried copper-molybdenum tailings, potassium feldspar, and waste glass were dry-milled for 1 hour respectively. According to the weight, 70 parts of copper-molybdenum tailings, 5 parts of potassium feldspar, flux (including 20 parts of waste glass and 5 parts of sodium carbonate), 1.0 part of foaming agent (the mass ratio of dolomite and sodium carbonate is 4:1), and 1.5 parts of foam stabilizer were weighed, all the materials were shaken and mixed, and then dry-milled for 2 hours. After the ball milling was completed, the mixture was sieved through a 200-mesh sieve, and the part under the sieve was taken and placed under 150°C for rapid drying for 2 hours, and then the dried mixed powder was evenly spread into the mold, vibrated, and the surface of the mixed powder was scraped flat. The mold filled with the mixed powder is sintered according to the temperature rising program. The specific temperature rising program is: room temperature-730℃, 10℃ / min; 730℃-900℃, 8℃ / min; keep warm at 900℃ for 8min; 900℃-940℃, 4℃ / min; keep warm at the sintering temperature for 20min, and process and cut after cooling to obtain copper-molybdenum tailings foamed ceramics. The properties of the prepared foamed ceramics are shown in Table 5.

[0074] Embodiments 10 to 11

[0075] The preparation steps are the same as those of Example 9, except that the sintering temperatures of Example 10 and Example 11 are adjusted to 970°C and 990°C, respectively. The properties are shown in Table 5.

[0076] Table 5. Performance of Examples 9 to 11

[0077] serial number Temperature(℃) <![CDATA[Density (kg / m 3 )]]> Compressive strength(MPa) Thermal conductivity [W / (m·K)] Example 9 940 849.3 19.25 0.099 Example 10 970 606.3 10.85 0.077 Embodiment 11 990 518.2 7.06 0.069

[0078] Table 5 shows that the sintering temperature gradually increases, while the density, compressive strength and thermal conductivity gradually decrease in the firing conditions of Example 9, Example 10 and Example 11, and Example 9, Example 10 and Example 11 meet the standards of density numbers of 800, 600 and 500, respectively.

[0079] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.

Claims

1. A foamed ceramic based on copper-molybdenum tailings, characterized in that: The raw materials include the following components by weight: 55-80 parts of copper-molybdenum tailings, 5-20 parts of potassium feldspar, 25 parts of flux, 0.5-1.5 parts of foaming agent and 1-3 parts of foam stabilizer; wherein: The flux is composed of sodium carbonate and waste glass, and the mass percentage of sodium carbonate in the flux is 12-32%; the foaming agent is composed of dolomite and silicon carbide; and the foam stabilizer is calcium phosphate.

2. The foamed ceramic according to claim 1, characterized in that: Measured by weight percentage, the main chemical components of the copper-molybdenum tailings are SiO2 66-71wt%, Al2O3 15-20wt%, CaO 0.5-3.0wt%, MgO 0.5-3.0wt%, K2O2-4wt%, Na2O 2-4wt%, Fe2O3 0.2-1.8wt%, CuO 0.06-0.15wt%, and MoO3 0.01-0.15wt%.

3. The foamed ceramic according to claim 1, characterized in that: In the foaming agent, the mass ratio of dolomite to silicon carbide is 4:1 to 5:

1.

4. The foamed ceramic according to claim 1, characterized in that: In the flux, the mass percentage of sodium carbonate is 15-25%.

5. The foamed ceramic according to claim 1, characterized in that: The density of the foamed ceramic based on copper-molybdenum tailings is 400-850 kg / m 3 ; The compressive strength is 4.77~19.25MPa; The thermal conductivity is less than 0.15W / (m·K).

6. A method for preparing a foamed ceramic based on copper-molybdenum tailings according to any one of claims 1 to 5, characterized in that: The following steps are involved: 1) Ball milling and mixing: dry-milling and mixing the dried copper-molybdenum tailings, potassium feldspar and waste glass respectively; then mixing the copper-molybdenum tailings, potassium feldspar and waste glass after ball milling with sodium carbonate, foaming agent and foam stabilizer, and then dry-milling and mixing, sieving and drying to obtain a mixed powder; 2) Evenly spreading the material: evenly spread the dry mixed powder obtained in step 1) into the mold, vibrate it, and scrape the surface of the mixed material flat; 3) Low-temperature firing: The mold filled with the mixed powder obtained in step 2) is sintered at 940-990° C., and cooled to obtain the copper-molybdenum tailings-based foamed ceramics.

7. The preparation method according to claim 6, characterized in that: In the step 1), the copper-molybdenum tailings, potassium feldspar and waste glass are dry-milled for 0.5 to 1 hour; then the copper-molybdenum tailings, potassium feldspar and waste glass after ball milling are shaken and mixed with sodium carbonate, a foaming agent and a foam stabilizer, and then dry-milled for 1 to 2 hours, passed through a 200-mesh sieve, and dried to obtain a mixed powder.

8. The preparation method according to claim 6, characterized in that: In the step 1), the drying condition is: drying at 130-150° C. for 1-3 hours.

9. The preparation method according to claim 6, characterized in that: In the step 3), the sintering time is 15 to 25 minutes.

10. The preparation method according to claim 6, characterized in that: The temperature rise program in step 3) is: room temperature - 730°C, The heating rate is 8-12℃ / min; 730℃-900℃, the heating rate is 8-10℃ / min; keep warm at 900℃ for 5-10min; 900℃~sintering temperature, heating rate is 3~4℃ / min.

Citation Information

Patent Citations

  • Foamed ceramic material and preparation method thereof

    CN102718547A

  • Method for producing light-weight inorganic plates by using industrial waste slag

    CN103172383A

  • Dry-hanging hollow ceramic slab prepared by using copper molybdenum tailing, and preparation method thereof

    CN103274669A

  • Method for preparing foamed ceramic thermal insulation material from red mud

    CN108503336A

  • Foamed ceramic heat preservation board

    CN109608167A

Cited By

  • Composite tailing foaming material prepared based on dual foaming system and preparation method of composite tailing foaming material