Conductive ceramic carbon fiber roller, preparation method and application
By forming a titanium oxide ceramic layer on the surface of the carbon fiber prepreg roller core and adding a metal transition layer and a sand layer, the problem of insufficient conductivity of carbon fiber materials is solved, and efficient anti-static performance in industries such as lithium batteries and chip manufacturing is achieved. The resistance of the resistance of the carbon fiber materials is achieved. The rate is stable and the process is simplified.
Patent Information
- Application Number
- CN202411182942.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Carbon fiber materials are inadequate when used in places where anti-static electricity is required, especially in the lithium battery film manufacturing and chip manufacturing industries.
The titanium oxide ceramic layer is formed on the surface of the carbon fiber prepreg roller core, and a metal transition layer and a sand layer are added between the carbon fiber prepreg roller core and the ceramic layer. The ceramic layer is formed through plasma spraying technology, and the metal transition layer is doped in the metal transition layer. Inorganic particles and organic resins to improve interfacial bonding and conductivity.
The excellent conductivity of carbon fiber rollers is achieved, the resistivity reaches 30Ω·cm and below, and the conductivity is stable, which meets high anti-static requirements, and simplifies the process and reduces production costs.
Smart Images

Figure CN118993769A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of material technology, and in particular to a conductive ceramic carbon fiber roller, a preparation method and application thereof. Background Art
[0002] The main part of the rollers commonly used in production lines is generally made of metal, which has a good static conductivity effect, but the cost is relatively high, the roller mass is large, and the rotational energy required for operation is also large, which is not conducive to sudden turns and stops. It is easy to corrode after long-term use, and long-term horizontal placement can easily cause the roller body to bend and deform, affecting the accuracy of the roller body.
[0003] Carbon fiber has many excellent properties such as high strength, high modulus, high temperature resistance, wear resistance, corrosion resistance, fatigue resistance, creep resistance, electrical conductivity, thermal conductivity and far infrared radiation. Carbon fiber tubes can be used in textile machinery, aluminum foil machinery, plastic film machinery, papermaking machinery, printing / dying machinery, to solve the problems of high cost of rollers made of metal, easy corrosion after long-term use, and easy bending and deformation of the roller body, which affects the accuracy of the roller body.
[0004] Therefore, when using carbon fiber as a roller, the carbon fiber will be modified and resin material will be added to the carbon fiber precursor. A ceramic coating is applied to the surface of the carbon fiber material. For example, CN101016614A discloses a process for spraying ceramic on the surface of an epoxy resin carbon fiber composite product, which includes the following steps: A. Roughening the surface of the epoxy resin-based carbon fiber composite product; B. Spraying a metal base layer on the roughened surface; C. Spraying ceramic powder on the surface of the metal base layer to form a ceramic coating. However, this will bring new problems. The carbon fiber precursor itself has good electrical conductivity, but its electrical conductivity is weaker than that of metal, and the resin material itself is not conductive. After the resin material fully infiltrates the carbon fiber precursor, if the latter can be evenly wrapped, the electrical conductivity of the manufactured carbon fiber roller will be greatly reduced or even completely lost. After the ceramic coating is applied to the surface, most of the ceramic coatings are not conductive, and cannot meet the requirements in places where anti-static is required, such as thin film manufacturing in the lithium battery industry and chip manufacturing industry. Summary of the invention
[0005] The purpose of the present invention is to solve the defect of insufficient antistatic ability of the above-mentioned carbon fiber material when used in places where antistatic is required, and to provide a conductive ceramic carbon fiber roller, preparation method and application, especially in the lithium battery film manufacturing and chip manufacturing industries, which have obvious advantages.
[0006] In a first aspect of the present invention, a conductive ceramic carbon fiber roller is provided, which adopts the following technical solution: A conductive ceramic carbon fiber roller comprises a carbon fiber prepreg roller core and a ceramic layer formed on the outer surface of the carbon fiber prepreg roller core, wherein the ceramic layer is a coating formed by titanium oxide, and the general formula of titanium oxide is: Ti n O 2n-1 (4≤n≤10).
[0007] In the above scheme, a conductive ceramic layer formed by titanium oxide is coated on the surface of the roller core formed by carbon fiber prepreg to give the carbon fiber roller antistatic properties. After testing, the resistivity of the roller surface can reach 30Ω·cm or less after spraying the conductive ceramic.
[0008] As mentioned in CN101016614A in the background technology, in order to solve the problem of easy deformation of epoxy resin-based carbon fiber composite materials and expand their scope of use, a ceramic layer is sprayed on the surface, and the high temperature resistance, wear resistance, heat insulation and other characteristics of ceramics are used to protect epoxy resin-based carbon fiber composite materials and their products. In this patent application technology, the antistatic properties of the material are not considered. However, most ceramics are not conductive and cannot give conductive properties to products.
[0009] Of course, in the prior art, there are also some conductive ceramics, such as metal ceramics. In the early stage of research and development, the inventors selected some common types of these conductive metal ceramics, including carbide-based metal ceramics, oxide-based metal ceramics, and nitride-based metal ceramics. However, after experiments, it was found that the conductivity of some ceramics could not achieve the expected effect, and they could not meet the requirements for lithium batteries, chips and other industries with high anti-static performance requirements. Some ceramics, such as WC-12Co metal ceramics, although the conductivity can meet the requirements, are found to have poor stability, especially after a period of use, the resistivity fluctuates significantly.
[0010] Therefore, the inventors expanded the scope of conductive ceramics and found that titanium oxide ceramics (Ti n O 2n-1 (4≤n≤10)), used on the surface of carbon fiber prepreg roller core, can give the carbon fiber roller excellent conductive properties and stable performance.
[0011] Preferably, a metal transition layer formed of metal powder is formed between the carbon fiber prepreg roll core and the ceramic layer. Directly spraying ceramic powder on the surface of the carbon fiber prepreg to form a ceramic layer will cause thermal stress to be generated when the temperature changes due to the difference in thermal barrier properties between the carbon fiber material and the ceramic material, which will affect the interface bonding strength and further cause the coating to crack or fall off: a poor interface bonding may be formed between the carbon fiber and the ceramic, affecting the overall performance of the surface ceramic coating. Adding a metal transition layer between the two is helpful to overcome the above problems to a certain extent.
[0012] Preferably, a sand layer is formed between the carbon fiber prepreg roll core and the metal transition layer. By providing the sand layer, the specific surface area of the carbon fiber prepreg roll core is increased, which is conducive to the stable formation of the subsequent coating.
[0013] Preferably, the sand layer is formed by spraying white corundum with a mesh size of 30 to 50.
[0014] Preferably, the metal powder used in the metal transition layer is doped with inorganic particles and organic resin. After adding a metal transition layer formed by pure metal powder between the carbon fiber prepreg roller core and the ceramic layer, although the problem of interface bonding can be solved to a certain extent, when forming the ceramic layer, the conductivity between different rollers in the same batch and between rollers in different batches is quite different, and the stability between batches is poor. The inventor speculates that this may be caused by the uneven distribution of ceramic powder caused by the spraying formation process of the surface ceramic layer. Attempts have been made to adjust the spraying process parameters, but the results have not been significantly improved. Therefore, it was considered whether it was due to the influence of the underlying metal transition layer. After a series of experiments, it was determined that the addition of the metal transition layer led to large differences in conductivity between different rollers in the same batch and between rollers in different batches. During the experiment, it was found that doping a small amount of inorganic particles and organic resin in the metal powder at the same time was conducive to greatly improving the problem of large differences in conductivity.
[0015] Preferably, the inorganic particles have a particle size of 50 nm to 150 nm.
[0016] Preferably, in the metal transition layer, the weight ratio of metal powder, inorganic particles and organic resin is 1:(0.1-0.15):(0.1-0.2).
[0017] Preferably, the inorganic particles are any one of silicon dioxide, titanium dioxide, aluminum oxide, calcium carbonate, etc., or a mixture of several of them.
[0018] Preferably, the organic resin is epoxy resin.
[0019] The second aspect of the present invention provides a method for preparing the above-mentioned conductive ceramic carbon fiber roller, comprising the following steps: (1) Providing a roller core made of carbon fiber prepreg; (2) Clean the surface of the roller core and form a sand layer by sandblasting; (3) spraying metal powder on the roller surface with the sand layer to form a metal powder layer; (4) Ceramic powder is sprayed on the roller surface on which the metal powder layer is formed to form a ceramic layer.
[0020] Preferably, in step (4), the ceramic layer is sprayed by plasma spraying equipment, and the spraying conditions are: spraying current 500-555A, main gas flow rate 25-32L / min, secondary gas flow rate 3-5.5L / min, and delivery amount 30-50g / min.
[0021] A third aspect of the present invention provides an application of the conductive ceramic carbon fiber roller for use in lithium battery film manufacturing or chip manufacturing.
[0022] By implementing the above technical solution, compared with the prior art, the present invention has the following advantages: 1. The present invention forms a ceramic layer composed of titanium oxide on the surface of the carbon fiber prepreg roller core, giving the roller surface excellent conductive properties.
[0023] 2. By forming a sand layer and a metal powder layer on the surface of the roller core before the ceramic layer is formed, the adhesion of the ceramic layer is improved, making the formation of the ceramic layer more stable.
[0024] 3. The stability of the conductive performance of the conductive ceramic carbon fiber roller is improved by targeted improvement of the composition of the metal powder layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a schematic diagram of the hierarchical structure of a conductive ceramic carbon fiber roller according to an embodiment of the present invention.
[0026] In the figure, 101 is a roller core, 102 is a metal powder layer, and 103 is a ceramic layer. DETAILED DESCRIPTION
[0027] The following describes the embodiments of the present invention by specific specific embodiments, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied by other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and embodiments can be combined with each other without conflict. The methods used in the embodiments of the present invention are all conventional methods unless otherwise specified.
[0028] Example 1 The present embodiment provides a conductive ceramic carbon fiber roller, comprising a carbon fiber prepreg roller core and a ceramic layer formed on the outer surface of the carbon fiber prepreg roller core, the ceramic layer is made of titanium dioxide Ti4O7 and is a coating formed by spraying using plasma spraying equipment, the spraying current is 550A, the main air flow rate is 30L / min, the secondary air flow rate is 4L / min, the delivery amount is 35g / min, and the coating thickness is 0.5mm.
[0029] Example 2 This embodiment provides a conductive ceramic carbon fiber roller, which is different from the embodiment 1 in that a layer of aluminum alloy coating with a thickness of 0.07 mm is first sprayed on the carbon fiber prepreg roller core, and then a ceramic layer is formed on the aluminum alloy coating. The aluminum alloy coating is formed by arc spraying, and the spraying conditions are current 100A, voltage 25V, and spraying distance 100mm. The ceramic layer is a coating formed by spraying titanium suboxide Ti4O7, with a spraying current of 550A, a primary gas flow rate of 30L / min, a secondary gas flow rate of 4L / min, a delivery amount of 35g / min, and a coating thickness of 0.5mm.
[0030] Example 3 This embodiment provides a conductive ceramic carbon fiber roller, which is different from the embodiment 2 in that 30-50 mesh white corundum is first sprayed on the carbon fiber prepreg roller core (the sandblasting pressure is 0.5MPa, and the sandblasting amount is 300g), and then a layer of aluminum coating with a thickness of 0.07mm is sprayed, and then a ceramic layer is formed on the aluminum coating. The aluminum alloy coating is formed by arc spraying, and the spraying conditions are current 100A, voltage 25V, and spraying distance 100mm. The ceramic layer is a coating formed by spraying titanium suboxide Ti4O7, the spraying current is 550A, the main gas flow rate is 30L / min, the secondary gas flow rate is 4L / min, the delivery amount is 35g / min, and the coating thickness is 0.5mm.
[0031] Example 4 The present embodiment provides a conductive ceramic carbon fiber roller, comprising a carbon fiber prepreg roller core, a metal powder layer formed on the outer surface of the carbon fiber prepreg roller core, and a ceramic layer formed on the outer surface of the metal powder layer, wherein the ceramic layer is a coating formed by spraying titanium suboxide Ti4O7, the spraying current is 550A, the main gas flow rate is 30L / min, the secondary gas flow rate is 4L / min, the delivery amount is 35g / min, and the coating thickness is 0.5mm. The thickness of the metal powder layer is 0.07mm. The raw materials of the metal powder layer are: 1 part by weight of aluminum powder, 0.1 part by weight of silicon dioxide particles, and 0.1 part by weight of epoxy resin powder. The particle size of the silicon dioxide particles is between 100-150nm. The metal powder coating is formed by arc spraying, and the spraying conditions are current 100A, voltage 25V, and spraying distance of 100mm.
[0032] The difference from Example 2 is that the coating material forming the metal powder is different.
[0033] Example 5 The present embodiment provides a conductive ceramic carbon fiber roller, comprising a carbon fiber prepreg roller core, a metal powder layer formed on the outer surface of the carbon fiber prepreg roller core, and a ceramic layer formed on the outer surface of the metal powder layer, wherein the ceramic layer is a coating formed by spraying titanium suboxide Ti4O7, the spraying current is 550A, the main gas flow rate is 30L / min, the secondary gas flow rate is 4L / min, the delivery amount is 35g / min, and the coating thickness is 0.5mm. The thickness of the metal powder layer is 0.07mm. The raw materials of the metal powder layer are: 1 part by weight of aluminum powder, 0.15 parts by weight of silicon dioxide particles, and 0.1 parts by weight of epoxy resin powder. The particle size of the silicon dioxide particles is between 100-150nm. The metal powder coating is formed by arc spraying, and the spraying conditions are current 100A, voltage 25V, and spraying distance of 100mm.
[0034] Example 6 The present embodiment provides a conductive ceramic carbon fiber roller, comprising a carbon fiber prepreg roller core, a metal powder layer formed on the outer surface of the carbon fiber prepreg roller core, and a ceramic layer formed on the outer surface of the metal powder layer, wherein the ceramic layer is a coating formed by spraying titanium suboxide Ti4O7, the spraying current is 550A, the main gas flow rate is 30L / min, the secondary gas flow rate is 4L / min, the delivery amount is 35g / min, and the coating thickness is 0.5mm. The thickness of the metal powder layer is 0.07mm. The raw materials of the metal powder layer are: 1 part by weight of aluminum powder, 0.15 parts by weight of silicon dioxide particles, and 0.2 parts by weight of epoxy resin powder. The particle size of the silicon dioxide particles is between 100-150nm. The metal powder coating is formed by arc spraying, and the spraying conditions are current 100A, voltage 25V, and spraying distance of 100mm.
[0035] Example 7 The present embodiment provides a conductive ceramic carbon fiber roller, comprising a carbon fiber prepreg roller core, a metal powder layer formed on the outer surface of the carbon fiber prepreg roller core, and a ceramic layer formed on the outer surface of the metal powder layer, wherein the ceramic layer is a coating formed by spraying titanium suboxide Ti4O7, the spraying current is 550A, the main gas flow rate is 30L / min, the secondary gas flow rate is 4L / min, the delivery amount is 35g / min, and the coating thickness is 0.5mm. The thickness of the metal powder layer is 0.07mm. The raw materials of the metal powder layer are: 1 part by weight of aluminum powder, 0.13 parts by weight of silicon dioxide particles, and 0.15 parts by weight of epoxy resin powder. The particle size of the silicon dioxide particles is between 100-150nm. The metal powder coating is formed by arc spraying, and the spraying conditions are current 100A, voltage 25V, and spraying distance 100mm.
[0036] Example 8 The present embodiment provides a conductive ceramic carbon fiber roller, comprising a carbon fiber prepreg roller core, a metal powder layer formed on the outer surface of the carbon fiber prepreg roller core, and a ceramic layer formed on the outer surface of the metal powder layer, wherein the ceramic layer is a coating formed by spraying titanium suboxide Ti4O7, the spraying current is 550A, the main gas flow rate is 30L / min, the secondary gas flow rate is 4L / min, the delivery amount is 35g / min, and the coating thickness is 0.5mm. The thickness of the metal powder layer is 0.07mm. The raw materials of the metal powder layer are: 1 part by weight of aluminum-magnesium alloy powder, 0.15 parts by weight of titanium dioxide particles, and 0.2 parts by weight of epoxy resin powder. The particle size of the silicon dioxide particles is between 50-100nm. The metal powder coating is formed by arc spraying, and the spraying conditions are current 100A, voltage 25V, and spraying distance 100mm.
[0037] Example 9 The present embodiment provides a conductive ceramic carbon fiber roller, comprising a carbon fiber prepreg roller core, a sand layer sprayed on the surface of the roller core, a metal powder layer formed on the surface of the sand layer, and a ceramic layer formed on the outer surface of the metal powder layer. The sand layer is formed by spraying 30-50 mesh white corundum. The ceramic layer is a coating formed by spraying titanium dioxide Ti4O7, with a spraying current of 550A, a main gas flow rate of 30L / min, a secondary gas flow rate of 4L / min, a delivery amount of 35g / min, and a coating thickness of 0.5mm. The thickness of the metal powder layer is 0.07mm. The raw materials of the metal powder layer are: 1 part by weight of aluminum-magnesium alloy powder, 0.15 parts by weight of titanium dioxide particles, and 0.2 parts by weight of epoxy resin powder. The particle size of the silicon dioxide particles is between 50-100nm. The metal powder coating is formed by arc spraying, and the spraying conditions are a current of 100A, a voltage of 25V, and a spraying distance of 100mm.
[0038] The average resistivity of the surface of the ceramic carbon fiber roller obtained in the above embodiments (just out of the factory and after 3 months of use) was tested using a resistivity tester. The test results are shown in Table 1 below (the resistivity in Table 1 is the average value obtained by selecting 5 ceramic carbon fiber rollers).
[0039] Table 1 Resistivity of the carbon fiber roller surface obtained in each example
[0040] From the results shown in Table 1, it can be seen that the surface resistivity of the ceramic carbon fiber roller obtained in each of the above embodiments is below 30Ω·cm at the initial stage of leaving the factory, which can meet the use of places with high antistatic requirements. In particular, in Examples 4 to 9, after adopting a specific metal powder layer, the resistivity is below 20Ω·cm at the initial stage of leaving the factory, which has a significant improvement and better antistatic performance. Among them, Example 7 optimizes the composition ratio of the metal powder layer, and the antistatic performance of the obtained ceramic carbon fiber roller is the best. From the resistivity after three months of use, the resistivity of the ceramic carbon fiber roller (Examples 1 and 2) corresponding to the metal powder layer formed by using conventional metal powder increases after three months, and the antistatic performance decreases. In the scheme of adding a sand layer (Example 3), it is alleviated to a certain extent, but the antistatic performance still decreases. The resistivity of the ceramic carbon fiber roller (Examples 4-9) corresponding to the specific metal powder layer of the present invention does not change significantly after three months, and the ceramic carbon fiber roller still has a relatively good antistatic effect. Although the sand layer is added in Example 9 compared with Example 8, it has no positive effect on the final effect. This shows that by adopting the specific metal powder layer of the present invention, the sand layer can be omitted, which is more conducive to simplifying the process and controlling the production cost.
[0041] In order to study the stability of the anti-static performance of the ceramic carbon fiber roller between batches, the resistivity of the ceramic carbon fiber rollers obtained from the same production batch and different production batches (the production conditions of different production batches are the same) of the above embodiments was also tested and analyzed. The results are shown in Table 2 (resistivity of the same production batch, the resistivity corresponding to 5 ceramic carbon fiber rollers) and Table 3 (resistivity between different production batches, three batches, the average value of 5 ceramic carbon fiber rollers selected from each production batch). Among them, the uniformity calculation formula is as follows: uniformity = [(maximum film thickness - minimum value) / (2*average film thickness)] * 100%, the smaller the uniformity, the more stable the resistivity, and vice versa, the greater the uniformity, the more unstable the resistivity.
[0042] Table 2 Resistivity of ceramic carbon fiber rollers from the same production batch
[0043] Table 3 Resistivity of ceramic carbon fiber rollers from different production batches
[0044] Comparative Example 1 This comparative example provides a conductive ceramic carbon fiber roller, which is different from Example 2 in that the ceramic layer is formed by spraying WC-12Co powder material.
[0045] Comparative Example 2 This comparative example provides a conductive ceramic carbon fiber roller, which is different from Example 2 in that the ceramic layer is formed by spraying WC-12Ni powder material.
[0046] Comparative Example 3 This comparative example provides a conductive ceramic carbon fiber roller, which is different from Example 2 in that the ceramic layer is formed by spraying Cr3C2-NiCr (75% (Cr3C2)-25% (NiCr)) powder material.
[0047] Comparative Examples 1-3 are several commonly used conductive metal ceramic powders purchased by the inventor from the market. A ceramic layer is formed on the metal powder coating formed on the surface of the carbon fiber prepreg roller core. The factory average resistivity of the ceramic carbon fiber roller surface obtained in Example 2 and each comparative example is tested. The test results are shown in Table 4 below (the resistivity in Table 4 is the average value obtained by selecting 5 ceramic carbon fiber rollers).
[0048] Table 4 Average resistivity of the surface of the ceramic carbon fiber roller obtained in Example 2 and each comparative example
[0049] As can be seen from Table 4, when the ceramic powder of the comparative example is used to form the ceramic layer, the resistivity of the corresponding ceramic carbon fiber roller obtained is significantly increased, and the requirement for high antistatic performance is not met.
Claims
1. A conductive ceramic carbon fiber roller, comprising a carbon fiber prepreg roller core and a ceramic layer formed on the outer surface of the carbon fiber prepreg roller core, characterized in that: The ceramic layer is a coating formed by titanium suboxide, and the general formula of titanium suboxide is: Ti n O 2n-1 (4≤n≤10).
2. A conductive ceramic carbon fiber roller according to claim 1, characterized in that: A metal transition layer formed of metal powder is also formed between the carbon fiber prepreg roller core and the ceramic layer.
3. A conductive ceramic carbon fiber roller according to claim 2, characterized in that: A sand layer is also formed between the carbon fiber prepreg roller core and the metal transition layer.
4. The conductive ceramic carbon fiber roller according to claim 3, characterized in that: The sand layer is formed by spraying white corundum with a mesh size of 30 to 50.
5. A conductive ceramic carbon fiber roller according to claim 1 or 2, characterized in that: The metal transition layer uses metal powder doped with inorganic particles and organic resin.
6. The conductive ceramic carbon fiber roller according to claim 5, characterized in that: The particle size of the inorganic particles is 50 nm to 150 nm.
7. The conductive ceramic carbon fiber roller according to claim 5, characterized in that: In the metal transition layer, the weight ratio of metal powder, inorganic particles and organic resin is 1:(0.1-0.15):(0.1-0.2).
8. The conductive ceramic carbon fiber roller according to claim 5, characterized in that: The inorganic particles are any one of silicon dioxide, titanium dioxide, aluminum oxide, and calcium carbonate, or a mixture of several thereof, and the organic resin is epoxy resin.
9. The method for preparing a conductive ceramic carbon fiber roller according to any one of claims 1 to 8, wherein: The steps include: S1 provides a roller core made of carbon fiber prepreg; S2. Clean the roller core surface and sandblast to form a sand layer; S3. Spraying metal powder on the roller surface to form a sand layer to form a metal powder layer; S4. Spraying ceramic powder on the roller surface having the metal powder layer formed thereon to form a ceramic layer.
10. Use of a conductive ceramic carbon fiber roller according to any one of claims 1 to 8, characterized in that: Used in lithium battery thin film manufacturing or chip manufacturing.
Citation Information
Patent Citations
Process of spraying ceramic on epoxy resin base carbon fiber composite material article surface
CN101016614A
Multi-layer fire-barrier systems
AU2004247667A1
C / Ti4O7 composite nanofiber based lithium-sulfur battery positive electrode material and preparation method therefor
CN105489863A
Lead carbon battery positive electrode additive and preparation method thereof
CN106997952A
Carbon fiber composite board and preparation method thereof
CN112339367A
Cited By
Carbon fiber material workpiece sprayed with stainless steel coating on surface and preparation method of carbon fiber material workpiece
CN119507221A