Fluorocarbon resin as well as preparation method and application thereof
The fluorocarbon resin generated by copolymerization has solved the problem of poor adhesion of existing fluorocarbon resins, achieved high adhesion and durability, and was suitable for a wider range of application fields.
Patent Information
- Application Number
- CN202411261781.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-22
AI Technical Summary
The existing fluorocarbon resins have problems such as poor stability, yellowing, high viscosity, difficulty in construction and poor adhesion during storage and use, resulting in poor bonding force on the substrate and easy peeling.
By copolymerizing the first monomer, the second monomer and the third monomer in the reactor in which the initiator and the organic solvent are present, the first monomer, the second monomer and the third monomer are copolymerized to produce a fluorocarbon resin with excellent bonding. The specific step includes selecting a carbon- C2-C12 aliphatic hydrocarbons of carbon double bonds and fluorine atoms are used as the first monomer, and a second monomer with carbon-carbon double bonds and a third monomer containing epoxy are used, and the reaction temperature and time are controlled to ensure fluorine carbon. High adhesion and durability of resin.
The prepared fluorocarbon resin has excellent adhesion and durability, and can effectively adhere to various substrates, improve the impact resistance and flexibility of the coating, adapt to the deformation and expansion of the substrate, and extend the coating. Service life.
Smart Images

Figure CN118994462A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of polymers, and more specifically to a polymerization method for preparing a fluorocarbon resin, a high-adhesive fluorocarbon resin synthesized by the method, and an adhesive product or a coating product synthesized using the high-adhesive fluorocarbon resin. Background Art
[0002] Fluorocarbon resin (FEVE) has a wide range of application prospects in the coating industry due to its excellent weather resistance and chemical resistance. For example, fluorocarbon resin coatings are widely used in the anti-corrosion field of steel structures such as building exterior walls, automobiles, ships, bridges, etc., providing protection and decorative effects for the surface of objects. However, the fluorocarbon resins in the prior art have poor storage stability, easy yellowing, high viscosity, difficult construction, poor adhesion, poor wetting and dispersibility of resin and pigment, and the poor adhesion is the most critical defect. The poor adhesion of fluorocarbon resins will lead to poor bonding between fluorocarbon resin coatings and substrates, coating difficulties, easy peeling and other problems. In order to solve this problem, major enterprises and scientific research institutions in this field have invested a lot of scientific research costs and energy to carry out long-term research and development, and have tried various improvements in fluorocarbon resin formulas and production processes, but have not been able to obtain any truly satisfactory results in this regard. Therefore, it is urgent to develop a high-adhesive fluorocarbon resin with excellent adhesion, and the coating prepared using this resin can be firmly bonded to the surface of various substrates (including metals, glass, tiles, etc.), so that the coating can resist erosion and damage from the external environment for a long time.
[0003] In view of the problems existing in the above-mentioned prior art, the inventors of the present application have unexpectedly developed a method for preparing fluorocarbon resin through extensive and in-depth research. The fluorocarbon resin prepared by this method has extremely excellent adhesion, and the coating prepared using the fluorocarbon resin has high adhesion and high durability. In addition, the coating has improved flexibility, so that it can adapt to the deformation and expansion of the substrate, improve the impact resistance of the coating, and make the fluorocarbon coating more durable and suitable for a wider range of applications. Summary of the invention
[0004] The first aspect of the present application provides a method for preparing a fluorocarbon resin, the method comprising: in a reactor in the presence of an initiator and an organic solvent, causing a raw material including a first monomer, a second monomer and a third monomer to undergo a copolymerization reaction to generate a fluorocarbon resin;
[0005] The first monomer is a C2-C12 aliphatic hydrocarbon containing at least one carbon-carbon double bond and at least one fluorine atom, and the first monomer optionally further contains one or more non-fluorine halogen atoms; the content of the first monomer is 25-65% by weight based on the total weight of the material in the reactor;
[0006] The second monomer has a structure as shown in Formula I, provided that the second monomer contains at least one carbon-carbon double bond:
[0007] R1-O-R2 formula I
[0008] wherein R1 and R2 are each independently selected from the group consisting of C1-C12 alkyl, C2-C12 alkenyl, C3-C12 cycloalkyl, C3-C12 cycloalkenyl, C6-C16 aralkyl, C1-C12 hydroxyalkyl, C2-C12 hydroxyalkenyl, C3-C12 hydroxycycloalkyl, C3-C12 hydroxycycloalkenyl, C2-C12 fatty alkanoyl, C6-C16 aromatic alkanoyl; and the content of the second monomer is 10-30% by weight based on the total weight of the materials in the reactor;
[0009] The third monomer has a structure shown in Formula II, provided that the third monomer contains at least one carbon-carbon double bond:
[0010] R3-OR 4 Formula II
[0011] Wherein R3 is selected from: C2-C12 alkenyl-acyl, C2-C12 aralkenyl-acyl, fluorinated C2-C12 alkenyl-acyl, fluorinated C2-C12 aralkenyl-acyl, C2-C12 alkenyl, fluorinated C2-C12 alkenyl; R4 is selected from: C1-C8 alkyl connected with at least one epoxy (C2-C5 alkyl), C3-C12 cycloalkyl connected with at least one epoxy (C2-C5 alkyl), C6-C12 aryl connected with at least one epoxy (C2-C5 alkyl); based on the total weight of the material in the reactor, the content of the third monomer is 0.1-10 weight%.
[0012] According to one embodiment of the present application, the first monomer is selected from one or more of the following: chlorotrifluoroethylene, tetrafluoroethylene, vinylidene fluoride, hexafluoropropylene, 2,3,3,3-tetrafluoropropylene, and octafluorobutene.
[0013] According to another embodiment of the present application, the second monomer is selected from one or more of the following: hydroxyethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, hydroxypentyl vinyl ether, hydroxyhexyl vinyl ether, cyclobutyl vinyl ether, cyclohexyl vinyl ether, cyclohexyl dimethyl divinyl ether, ethyl vinyl ether, propyl vinyl ether, butyl vinyl ether, pentyl vinyl ether, allyl vinyl ether, vinyl benzoate, vinyl acetate, propionic acid vinyl ether, vinyl butyrate, vinyl valerate, vinyl hexanoate, and vinyl nonanoate.
[0014] According to another embodiment of the present application, the third monomer is selected from one or more of the following: glycidyl (meth)acrylate, allyl glycidyl ether, tetrafluorovinyl glycidyl ether, 2,3-epoxypropyl acrylate, and tetrafluorovinyl-2,3-epoxypropyl ether.
[0015] According to another embodiment of the present application, based on the total weight of the materials in the reactor, the content of the first monomer is 35-55% by weight, the content of the second monomer is 15-25% by weight, and the content of the third monomer is 0.5-5% by weight.
[0016] According to another embodiment of the present application, the organic solvent is selected from one or more of the following: ethyl acetate, propyl acetate, butyl acetate, ethyl valerate, toluene, xylene, acetone, methyl ethyl ketone, propylene glycol methyl ether acetate. According to another embodiment of the present application, based on the total weight of the materials in the reactor, the content of the organic solvent is 40-60% by weight.
[0017] According to another embodiment of the present application, the organic solvent is a mixture of ethyl acetate and methyl ethyl ketone in a weight ratio of 3:1 to 7:1, or a mixture of butyl acetate and xylene in a weight ratio of 3:1 to 7:1, or any one of pure xylene, pure butyl acetate, pure methyl ethyl ketone, and pure propylene glycol methyl ether acetate, or a mixture in any proportion.
[0018] According to another embodiment of the present application, the initiator is selected from one or more of the following: tert-butyl peroxypivalate, diisopropyl peroxydicarbonate, tert-amyl peroxypivalate, 3-hydroxy-1,1-dimethylbutyl peroxyneodecanoic acid, tert-butyl peroxyneodecanoate; based on the total weight of the materials in the reactor, the content of the initiator is 0.01-2 weight %.
[0019] According to another embodiment of the present application, during the copolymerization reaction, the reactor further contains an auxiliary agent, which is selected from one or more of the following: sodium carbonate, light stabilizer 292, zinc oxide, magnesium oxide; based on the total weight of the materials in the reactor, the content of the auxiliary agent is 0.05-1% by weight.
[0020] According to another embodiment of the present application, the temperature of the copolymerization reaction is 50-90° C., and the duration of the copolymerization reaction is 2-12 hours.
[0021] According to another embodiment of the present application, during the copolymerization reaction, at least a portion of at least one of the first monomer, the second monomer and the third monomer is continuously added into the reactor.
[0022] The second aspect of the present application provides a fluorocarbon resin, whose main chain contains a first copolymer unit, a second copolymer unit and a third copolymer unit. Based on the total weight of the fluorocarbon resin, the content of the first copolymer unit is 25-80% by weight, the content of the second copolymer unit is 10-60% by weight, the content of the third copolymer unit is 0.1-20% by weight, and the number average molecular weight of the fluorocarbon resin is 8000-40000 g / mol.
[0023] According to another embodiment of the present application, the first copolymerized unit is derived from a first monomer, the first monomer is a C2-C12 aliphatic hydrocarbon containing at least one carbon-carbon double bond and at least one fluorine atom, and the first monomer optionally further contains one or more non-fluorine halogen atoms.
[0024] According to another embodiment of the present application, the second copolymerized unit is derived from a second monomer, and the second monomer has a structure shown in Formula I, provided that the second monomer contains at least one carbon-carbon double bond:
[0025] R1-O-R2 formula I
[0026] Wherein R1 and R2 are each independently selected from: C1-C12 alkyl, C2-C12 alkenyl, C3-C12 cycloalkyl, C3-C12 cycloalkenyl, C6-C16 aralkyl, C1-C12 hydroxyalkyl, C2-C12 hydroxyalkenyl, C3-C12 hydroxycycloalkyl, C3-C12 hydroxycycloalkenyl, C2-C12 fatty alkanoyl, C6-C16 aromatic alkanoyl.
[0027] According to another embodiment of the present application, the third copolymerized unit is derived from a third monomer, and the third monomer has a structure shown in Formula II, provided that the third monomer contains at least one carbon-carbon double bond:
[0028] R3-OR 4 Formula II
[0029] Wherein R3 is selected from: C2-C12 alkenyl-acyl, C2-C12 aralkenyl-acyl, fluorinated C2-C12 alkenyl-acyl, fluorinated C2-C12 aralkenyl-acyl, C2-C12 alkenyl, fluorinated C2-C12 alkenyl; R4 is selected from: C1-C8 alkyl connected with at least one epoxy (C2-C5 alkyl), C3-C12 cycloalkyl connected with at least one epoxy (C2-C5 alkyl), C6-C12 aryl connected with at least one epoxy (C2-C5 alkyl).
[0030] According to another embodiment of the present application, the fluorocarbon resin is prepared by the method of the present invention.
[0031] The third aspect of the present application provides a coating product or an adhesive product, which contains the fluorocarbon resin of the present application.
[0032] In the following specific implementation section, the method, fluorocarbon resin and application of the present application are further introduced in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The reactor used for copolymerization reaction in the examples of the present application is shown;
[0034] Figure 2 The universal tensile testing machine used to detect the strength of the copolymerization product in the examples of the present application is shown;
[0035] Figure 3 The graph shows a test curve of the molecular weight of the copolymerization product prepared in the example of the present application detected by gel permeation chromatography. DETAILED DESCRIPTION
[0036] "Range" disclosed herein is in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges that can be defined in this way are inclusive and combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, a range of 60-120 and 80-110 is listed for a particular parameter, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.
[0037] In this application, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations.
[0038] In this application, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.
[0039] In this application, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0040] In this application, if there is no special explanation, the "including" mentioned herein means open or closed. For example, the "including" may mean that other components not listed may also be included, or only the listed components may be included.
[0041] One of the innovations of the present invention is that, through the design of special and carefully selected comonomer types and relative contents, the final fluorocarbon resin unexpectedly exhibits significantly improved adhesion, and the coating prepared using the fluorocarbon resin has high adhesion and high durability, and also has improved coating flexibility, enabling it to adapt to the deformation and expansion of the substrate, thereby improving the impact resistance of the coating.
[0042] Another innovation of the present invention is that during the copolymerization reaction using the above-mentioned specially designed comonomers, at least a portion of at least one of the various comonomers used is gradually and continuously added to the reactor, thereby avoiding the problem of explosion and more effectively controlling the molecular weight distribution of the fluorocarbon resin product, further significantly improving the product quality of the fluorocarbon resin.
[0043] According to one embodiment of the present application, a method for synthesizing a high-adhesion fluorocarbon resin is provided. Specifically, the adhesion of the fluorocarbon resin is characterized by the adhesion of a coating prepared from the fluorocarbon resin on a substrate. For example, the adhesion is ≥6MPa, preferably ≥7MPa, more preferably ≥8MPa, further preferably ≥9MPa, further preferably ≥10MPa, and in the most preferred case can reach above 13MPa. The adhesion of the coating on the substrate can be tested according to the standard method GB / T 5210-2006 "Pull-off adhesion test for paints and varnishes".
[0044] According to one embodiment of the present application, the method for preparing the high-adhesion fluorocarbon resin comprises the following steps: in a reactor, in the presence of an initiator and an organic solvent, copolymerizing raw materials including a first monomer, a second monomer and a third monomer to generate a fluorocarbon resin.
[0045] According to one embodiment of the present application, the first monomer is a C2-C12 aliphatic hydrocarbon containing at least one carbon-carbon double bond and at least one fluorine atom, and the first monomer optionally contains one or more non-fluorine halogen atoms; for example, a C2-C10 aliphatic hydrocarbon containing at least one carbon-carbon double bond and at least one fluorine atom, or a C2-C8 aliphatic hydrocarbon containing at least one carbon-carbon double bond and at least one fluorine atom, or a C2-C6 aliphatic hydrocarbon containing at least one carbon-carbon double bond and at least one fluorine atom. For example, the aliphatic hydrocarbon may contain one, two, three or four carbon-carbon double bonds, preferably one or two carbon-carbon double bonds. According to a specific embodiment of the present application, the first monomer may be substituted by one or more fluorine atoms, for example, it may be monofluoro, polyfluoro or perfluoro, and as mentioned above, it may also be substituted by one or more other halogen atoms (such as chlorine, bromine or iodine, preferably chlorine atom) while being fluorinated. For example, the first monomer used in the present invention is selected from one or more of the following: trifluorochloroethylene, tetrafluoroethylene, vinylidene fluoride, hexafluoropropylene, 2,3,3,3-tetrafluoropropylene, octafluorobutene. The first monomer may be introduced into the reactor in gaseous or liquid form, preferably in the form of a gaseous compound.
[0046] According to another embodiment of the present application, based on the total weight of the materials in the reactor (that is, based on the total weight of the first monomer, the second monomer, the third monomer, the organic solvent, the initiator, the auxiliary agent, and any other possible reaction-related components added to the reactor during the entire reaction process), the content of the first monomer is 25-65% by weight, for example, the monomer is within the numerical range obtained by combining any two of the following end values: 25% by weight, 26% by weight, 27% by weight, 28% by weight, 30% by weight, 32% by weight, 35% by weight, 38% by weight, 40% by weight, 45% by weight, 50% by weight, 60% by weight, 65% by weight; preferably 35-55% by weight.
[0047] According to one embodiment of the present application, the second monomer has a structure shown in Formula I, provided that the second monomer contains at least one carbon-carbon double bond:
[0048] R1-O-R2 formula I
[0049] According to one embodiment of the present application, the second monomer contains one, two, three or four carbon-carbon double bonds, preferably one or two carbon-carbon double bonds. According to one embodiment of the present application, in Formula I, R1 and R2 are each independently selected from the group consisting of: C1-C12 alkyl, C2-C12 alkenyl, C3-C12 cycloalkyl, C3-C12 cycloalkenyl, C6-C16 aralkyl, C1-C12 hydroxyalkyl, C2-C12 hydroxyalkenyl, C3-C12 hydroxycycloalkyl, C3-C12 hydroxycycloalkenyl, C2-C12 fatty alkanoyl, C6-C16 aromatic alkanoyl; for example, R1 and R2 are each independently selected from the group consisting of: C1-C6 alkyl, C2-C6 alkenyl, C3-C6 cycloalkyl, C3-C6 cycloalkenyl, C6-C12 aralkyl, C1-C6 hydroxyalkyl, C2-C6 hydroxyalkenyl, C3-C6 hydroxycycloalkyl, C3-C6 hydroxycycloalkenyl, C2-C7 fatty alkanoyl, C6-C13 aromatic alkanoyl. According to a specific embodiment of the present application, the second monomer is selected from one or more of the following: hydroxyethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, hydroxypentyl vinyl ether, hydroxyhexyl vinyl ether, cyclobutyl vinyl ether, cyclohexyl vinyl ether, cyclohexyl dimethyl divinyl ether, ethyl vinyl ether, propyl vinyl ether, butyl vinyl ether, pentyl vinyl ether, allyl vinyl ether, vinyl benzoate, vinyl acetate, propionic acid vinyl ether, vinyl butyrate, vinyl valerate, vinyl caproate, vinyl nonanoate. The second monomer is preferably input into the reactor in liquid form.
[0050] According to one embodiment of the present application, based on the total weight of the material in the reactor, the content of the second monomer is 10-30 weight %, for example, the monomer is within the numerical range obtained by combining any two of the following end values: 10 weight %, 12 weight %, 14 weight %, 15 weight %, 17 weight %, 18 weight %, 20 weight %, 22 weight %, 25 weight %, 27 weight %, 28 weight %, 30 weight %; preferably 15-25 weight %.
[0051] According to one embodiment of the present application, the third monomer has a structure shown in Formula II, provided that the third monomer contains at least one carbon-carbon double bond:
[0052] R3-O-R4 Formula II
[0053] According to one embodiment of the present application, the third monomer contains one, two, three or four carbon-carbon double bonds, preferably one or two carbon-carbon double bonds.
[0054] According to one embodiment of the present application, in formula II, R3 is selected from: C2-C12 alkenyl-acyl, C6-C16 aralkenyl-acyl, fluorinated C2-C12 alkenyl-acyl, fluorinated C6-C16 aralkenyl-acyl, C2-C12 alkenyl, fluorinated C2-C12 alkenyl; for example, R3 is selected from: C2-C6 alkenyl-acyl, C6-C12 aralkenyl-acyl, fluorinated C2-C6 alkenyl-acyl, fluorinated C6-C12 aralkenyl-acyl, C2-C6 alkenyl, fluorinated C2-C6 alkenyl.
[0055] According to one embodiment of the present application, in formula II, R4 is selected from: C1-C8 chain alkyl connected to at least one epoxy (C2-C5 alkyl), C3-C12 cycloalkyl connected to at least one epoxy (C2-C5 alkyl), C6-C12 aryl connected to at least one epoxy (C2-C5 alkyl); for example, R4 is selected from: C1-C6 chain alkyl connected to at least one epoxy (C2-C5 alkyl), C3-C8 cycloalkyl connected to at least one epoxy (C2-C5 alkyl), C6-C12 aryl connected to at least one epoxy (C2-C5 alkyl). The epoxy C2-C5 alkyl described above in R4 represents a group containing one ring oxygen atom and 2 to 5 ring carbon atoms, such as ethylene oxide, propylene oxide, butylene oxide, and pentyl oxide. According to an exemplary embodiment, the R4 contains one, two or three epoxy C2-C5 alkyl groups, preferably one ethylene oxide.
[0056] According to an exemplary embodiment of the present application, the third monomer is selected from one or more of the following: (meth) glycidyl acrylate, allyl glycidyl ether, tetrafluorovinyl glycidyl ether, 2,3-epoxypropyl acrylate, tetrafluorovinyl-2,3-epoxypropyl ether. The "glycidyl" in the glycidyl ether / ester described above is also called "1,2-epoxypropoxy", which has the following structural formula a; and the 2,3-epoxypropoxy contained in the latter two compounds has the following structural formula b, where "*" indicates that the 1,2- or 2,3-epoxypropoxy is connected to other parts of the third monomer through a covalent bond.
[0057]
[0058] According to one embodiment of the present application, based on the total weight of the material in the reactor, the content of the third monomer is 0.1-10% by weight, for example, the monomer is within the numerical range obtained by combining any two of the following end values: 0.1% by weight, 0.2% by weight, 0.3% by weight, 0.5% by weight, 0.7% by weight, 0.8% by weight, 1% by weight, 1.2% by weight, 1.5% by weight, 1.8% by weight, 2% by weight, 2.2% by weight, 2.5% by weight, 2.8% by weight, 3% by weight, 4% by weight, 5% by weight, 6% by weight, 7% by weight, 8% by weight, 9% by weight, 10% by weight; preferably 0.5-5% by weight.
[0059] According to one embodiment of the present application, the organic solvent is selected from one or more of the following: ethyl acetate, propyl acetate, butyl acetate, ethyl valerate, toluene, xylene, acetone, methyl ethyl ketone, propylene glycol methyl ether acetate. According to a preferred embodiment of the present application, the organic solvent is a mixture of the above two solvents, for example, a mixture of ethyl acetate and methyl ethyl ketone, the weight ratio of which is 3:1 to 7:1, for example, it can be 4:1 to 6:1; or a mixture of butyl acetate and xylene, the weight ratio of which is 3:1 to 7:1, for example, it can be 4:1 to 6:1. According to another embodiment of the present application, the organic solvent is pure xylene, pure butyl acetate, pure methyl ethyl ketone, pure propylene glycol methyl ether acetate, or a mixture of any two or more of the above solvents in any proportion.
[0060] According to one embodiment of the present application, based on the total weight of the material in the reactor, the content of the organic solvent is 40-60% by weight, for example, the organic solvent is within the numerical range obtained by combining any two of the following end values: 40% by weight, 42% by weight, 44% by weight, 45% by weight, 46% by weight, 48% by weight, 50% by weight, 51% by weight, 52% by weight, 55% by weight, 57% by weight, 58% by weight, 60% by weight; preferably 45-55% by weight.
[0061] According to one embodiment of the present application, the initiator is selected from one or more of the following: tert-butyl peroxypivalate, diisopropyl peroxydicarbonate, tert-amyl peroxypivalate, 3-hydroxy-1,1-dimethylbutyl peroxyneodecanoic acid, and tert-butyl peroxyneodecanoate.
[0062] According to a specific embodiment of the present application, based on the total weight of the materials in the reactor, the content of the initiator is 0.01-2 weight %; for example, the initiator is within the numerical range obtained by combining any two of the following end values: 0.01 weight %, 0.02 weight %, 0.05 weight %, 0.08 weight %, 0.1 weight %, 0.2 weight %, 0.3 weight %, 0.4 weight %, 0.5 weight %, 0.8 weight %, 1 weight %, 1.2 weight %, 1.5 weight %, 1.8 weight %, 2 weight %; preferably 0.5-1 weight %.
[0063] In the method of the present invention, one or more other auxiliary agents may be added to the reaction system as needed. For example, according to a specific embodiment of the present application, the auxiliary agent is selected from one or more of the following: light stabilizer 292, sodium carbonate, zinc oxide, magnesium oxide, etc. These auxiliary agents are used as acid binding agents in the reaction system to remove HF generated during the synthesis of the fluororesin, thereby improving the conversion rate of the monomer.
[0064] According to one embodiment of the present application, during the polymerization reaction, at least a portion (e.g., 50%, 60%, 70%, 80%, 90% or 100%) of any one, two or three of the first monomer, the second monomer and the third monomer can be gradually added to the reactor, preferably continuously added to the reactor. For example, before starting the reaction, a portion of any one, two or three of the first monomer, the second monomer and the third monomer is added to the reactor at one time, and then the remaining portion is continuously added to the reactor during the polymerization reaction. According to another exemplary embodiment of the present application, all materials of any one, two or three of the first monomer, the second monomer and the third monomer are continuously added to the reactor during the polymerization reaction. According to a preferred embodiment of the present application, before starting the reaction, a portion (preferably 5-40%, more preferably 10-25%) of the first monomer is first added to the reactor at one time, and then during the polymerization reaction, the remaining first monomer, and all of the second monomer and all of the third monomer are gradually added to the reactor.
[0065] According to an exemplary embodiment of the present application, the temperature of the copolymerization reaction is 50-90° C., and the duration of the copolymerization reaction is 2-12 hours.
[0066] According to an exemplary embodiment of the present application, the method of the present invention can be carried out in the following manner:
[0067] Step 1: First, add the organic solvent and auxiliary agent (if used) into the reaction kettle and start stirring.
[0068] Step 2: The reactor is evacuated to remove the air therein, and then the atmosphere in the reactor is replaced with nitrogen. If necessary, the above-mentioned evacuation-nitrogen replacement steps can be repeated until the oxygen content in the reactor is less than 20ppm, which is then judged as qualified. After passing the test, the reactor is evacuated again, and then a portion of the first monomer is charged into the reactor; for example, in this step 2, 5-40% of the first monomer is charged, preferably 15-25% of the first monomer is charged, and the remaining monomer is continuously charged into the reactor in the subsequent steps (such as step 3).
[0069] Step 3: In step 3, a first-stage copolymerization reaction occurs. In this step, the reactor is heated to a first reaction temperature, such as 50-65°C, preferably 55-60°C, and then part or all of the initiator is added to the reactor. The added initiator can be added all at once, or can be added gradually in a continuous or intermittent manner. Subsequently, the first monomer, the second monomer, and the third monomer are added to the reactor in a continuous manner, and the three monomers are maintained at a constant rate during the addition process, so that the three monomers are added in substantially the same time. According to one embodiment of the present application, the addition rate of the three monomers here is designed according to the percentage of each of the three monomer raw materials described above in the reaction raw materials. According to one embodiment of the present application, the first monomer, the second monomer, and the third monomer are added within 2-8 hours, preferably within 2-6 hours.
[0070] Step 4: After all the first monomer, the second monomer and the third monomer are added to the reactor in step 3, the reactor is heated to a second reaction temperature, such as 70-90°C, preferably 75-85°C; in this step, an initiator is added to the reactor, and the added initiator can be added all at once or gradually added in a continuous or intermittent manner. The reaction is continued at the second reaction temperature for 2-4 hours, such as 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours.
[0071] Step 5: After the reaction is completed, the reactor is cooled, opened and the material is discharged to obtain a crude product.
[0072] Step 6: The crude product is post-processed to obtain the high-adhesive fluorocarbon resin of the present application; the post-processing includes concentration, filtration, etc.
[0073] According to one embodiment of the present application, in the above steps 3-4, the pressure in the reactor is maintained at 0.2-1MPa, such as 0.2MPa, or 0.3MPa, or 0.4MPa, or 0.5MPa, or 0.6MPa, or 0.7MPa, or 0.8MPa, or 0.9MPa, or 1MPa, preferably 0.4-0.6MPa. According to a preferred embodiment of the present application, the above pressure in the reactor during the reaction process is mainly provided by the gaseous first monomer, and at the above reaction temperature, the liquid comonomer and solvent with a lower boiling point will also contribute a small amount to the pressure in the reactor.
[0074] According to one embodiment of the present application, the main chain of the fluorocarbon resin synthesized by the method of the present invention is mainly formed by the addition polymerization of the carbon-carbon double bonds of the first monomer, the second monomer and the third monomer, and the other groups of the three monomers except the carbon-carbon double bonds are attached to the main chain of the fluorocarbon resin or included in the main chain. According to one embodiment of the present application, based on the total weight of the fluorocarbon resin, the content of the first copolymerization unit formed by the first monomer is 25-80 weight % (for example, 30 weight %, 35 weight %, 40 weight %, 45 weight %, 50 weight %, 55 weight %, 60 weight %, 65 weight %, 70 weight %, 75 weight %, 80 weight %), and the content of the second copolymerization unit formed by the second monomer is 10-60 weight % (for example, 10 weight %, 15 weight %, 20 weight %, 25 weight %, 30 weight %, 35 weight %, 40 weight %, 45 weight %, 50 weight %, 55 weight %, 60 weight %, 65 weight %, 70 weight %, 75 weight %, 80 weight %). %, 60 wt %), and the content of the third copolymerized unit formed by the third monomer is 0.1-20 wt % (for example, 0.1 wt %, 0.2 wt %, 0.5 wt %, 0.8 wt %, 1 wt %, 1.2 wt %, 1.5 wt %, 1.8 wt %, 2 wt %, 2.2 wt %, 2.5 wt %, 2.8 wt %, 3 wt %, 3.2 wt %, 3.5 wt %, 3.5 wt %, 4 wt %, 5 wt %, 6 wt %, 7 wt %, 8 wt %, 9 wt %, 10 wt %, 12 wt %, 13 wt %, 15 wt %, 18 wt %, 20 wt %).
[0075] During the polymerization reaction, the residues of the initiators mentioned above will also be incorporated into the main chain of the polymer being formed, and eventually become part of the fluorocarbon resin, for example, as being connected to the end of the main chain, located in the middle of the main chain, or connected to the main chain as a side chain. In addition, during the polymerization reaction, the above-mentioned organic solvents may also become part of the fluorocarbon resin through chain transfer reactions, for example, as being connected to the end of the main chain, located in the middle of the main chain, or connected to the main chain as a side chain. However, compared with the content of the above-mentioned comonomers, the content of the part derived from the initiator and the organic solvent in the fluorocarbon resin is very low.
[0076] According to one embodiment of the present application, the number average molecular weight of the fluorocarbon resin is 8000 to 40000 g / mol.
[0077] The fluorocarbon resin of the present application can be used to formulate a coating composition or an adhesive composition, for example, based on the total weight of the coating or adhesive, the fluorocarbon resin content therein is 10-80% by weight, for example, 15-60% by weight, or 20-50% by weight, or 25-40% by weight, or 30-35% by weight, or within the numerical range obtained by combining any two of the above end values.
[0078] The advantage of the present invention is that, by specially designing the raw materials of the comonomers for preparing the fluorocarbon resin, a highly adhesive fluorocarbon resin is unexpectedly synthesized, and the coating prepared by using the fluorocarbon resin exhibits extremely excellent bonding with the substrate, improving the adhesion and durability of the coating. The inventor of the present invention has found through research that when the relative contents of the first monomer, the second monomer and the third monomer are not within the weight percentage range defined by the present invention, the obtained fluorocarbon resin coating will become significantly brittle, difficult to coat and poor in adhesion.
[0079] In addition, the applicant has further discovered through further research that in the process of copolymerization using the above-mentioned specially designed comonomers, at least a portion of at least one of the various comonomers used is gradually and continuously added to the reactor, thereby avoiding the problem of explosion and more effectively controlling the molecular weight distribution of the fluorocarbon resin product, further significantly improving the product quality of the fluorocarbon resin.
[0080] The method of the present application is specifically described in the following examples, the purpose of which is to better understand the content of the present application. It should be understood that these examples are merely illustrative and not restrictive. The reagents used in the examples, unless otherwise specified, are conventionally purchased from the market and used directly without further purification. The methods and conditions used in the examples, unless otherwise specified, are conventional methods and conditions.
[0081] Example
[0082] Example 1
[0083] This example uses Figure 1 The reactor shown is used for carrying out polymerization reaction. The reactor is equipped with a stirring device, a vacuum device, a heating and temperature control device, a gas / liquid / solid feeding device, and is connected with a nitrogen cylinder and a gas-phase monomer cylinder.
[0084] First, add 1200g of butyl acetate solvent and 5g of sodium carbonate auxiliary agent into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of chlorotrifluoroethylene into the reactor.
[0085] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-butyl peroxypivalate as an initiator was added to the reactor. Subsequently, 450 g of vinyl acetate, 150 g of hydroxybutyl vinyl ether, 50 g of glycidyl methacrylate and 600 g of chlorotrifluoroethylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0086] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 1 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0087] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated using a rotary evaporator at 70° C. and −0.09 MPa, filtered using a plate filter, and then a diluting solvent is added to the obtained solid material to obtain a fluorocarbon resin solution with a solid content of 50 wt%.
[0088] The molecular weight of the fluorocarbon resin prepared in this embodiment was detected by gel permeation chromatography (GPC). The GPC spectrum is shown in FIG. Figure 3 As shown, the measured number average molecular weight is 15409 g / mol.
[0089] According to the coating formula shown in Table 1 below, the fluorocarbon resin of this embodiment is used to prepare the coating. Figure 2 The universal tensile testing machine shown was used to test the adhesion of paints and varnishes on the substrate according to the standard method GB / T 5210-2006 "Paint and varnish adhesion test by pull-off method". The test results are summarized in Table 2.
[0090] Table 1 Coating formula
[0091] Components Effect of ingredients Weight FEVE Fluorocarbon resin 55 PMA Solvent 1 10 BAC Solvent 2 8.1 BYK-163 Dispersants 1 6900-20X Polyamide wax paste 0.6 Byk361N Leveling agent 0.2 6500 Defoaming agent 0.1 R-960 Titanium dioxide 25 100
[0092] Example 2
[0093] This example uses the same reaction equipment as Example 1.
[0094] First, add 900g of butyl acetate and 300g of xylene as solvent and 5g of sodium carbonate as auxiliary agent to the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of chlorotrifluoroethylene into the reactor.
[0095] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-butyl peroxypivalate as an initiator was added to the reactor. Subsequently, 450 g of vinyl acetate, 150 g of hydroxybutyl vinyl ether, 50 g of glycidyl methacrylate and 600 g of chlorotrifluoroethylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0096] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0097] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution with a solid content of 50 wt%.
[0098] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 12485 g / mol.
[0099] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0100] Example 3
[0101] This example uses the same reaction equipment as Example 1.
[0102] First, add 1200g of butyl acetate solvent and 5g of sodium carbonate auxiliary agent into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of tetrafluoroethylene into the reactor.
[0103] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-butyl peroxypivalate as an initiator was added to the reactor. Subsequently, 450 g of vinyl acetate, 150 g of hydroxybutyl vinyl ether, 50 g of glycidyl methacrylate and 600 g of tetrafluoroethylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0104] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0105] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution with a solid content of 50 wt%.
[0106] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 17380 g / mol.
[0107] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0108] Example 4
[0109] This example uses the same reaction equipment as Example 1.
[0110] First, add 1200g of butyl acetate solvent and 5g of sodium carbonate auxiliary agent into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of hexafluoropropylene into the reactor.
[0111] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-butyl peroxypivalate as an initiator was added to the reactor. Subsequently, 450 g of vinyl acetate, 150 g of hydroxybutyl vinyl ether, 50 g of glycidyl methacrylate and 600 g of hexafluoropropylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0112] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0113] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution with a solid content of 50 wt%.
[0114] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 16320 g / mol.
[0115] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0116] Example 5
[0117] This example uses the same reaction equipment as Example 1.
[0118] First, add 1200g of butyl acetate solvent and 5g of sodium carbonate auxiliary agent into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of chlorotrifluoroethylene into the reactor.
[0119] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-amyl peroxide pivalate as an initiator was added to the reactor. Subsequently, 450 g of ethyl vinyl ether, 150 g of hydroxybutyl vinyl ether, 50 g of glycidyl methacrylate and 600 g of chlorotrifluoroethylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0120] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-amyl peroxide pivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0121] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution with a solid content of 50 wt%.
[0122] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 22143 g / mol.
[0123] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0124] Example 6
[0125] This example uses the same reaction equipment as Example 1.
[0126] First, add 1200g of butyl acetate solvent and 5g of sodium carbonate auxiliary agent into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of chlorotrifluoroethylene into the reactor.
[0127] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-butyl peroxypivalate as an initiator was added to the reactor. Subsequently, 450 g of vinyl acetate, 150 g of hydroxybutyl vinyl ether, 50 g of tetrafluoroethylene glycidyl ether and 600 g of chlorotrifluoroethylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0128] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0129] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution with a solid content of 50 wt%.
[0130] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 26780 g / mol.
[0131] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0132] Example 7
[0133] This example uses the same reaction equipment as Example 1.
[0134] First, add 1200g of solvent xylene and 5g of auxiliary agent sodium carbonate into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of trifluorochloroethylene into the reactor.
[0135] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-butyl peroxypivalate as an initiator was added to the reactor. Subsequently, 150 g of hydroxybutyl vinyl ether, 250 g of cyclohexyl dimethanol divinyl ether, 200 g of ethyl vinyl ether, 50 g of allyl glycidyl ether and 600 g of chlorotrifluoroethylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0136] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0137] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution with a solid content of 50 wt%.
[0138] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 31130 g / mol.
[0139] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0140] Example 8
[0141] This example uses the same reaction equipment as Example 1.
[0142] First, add 1200g of xylene solvent and 5g of sodium carbonate auxiliary agent into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of tetrafluoroethylene into the reactor.
[0143] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-butyl peroxypivalate as an initiator was added to the reactor. Subsequently, 150 g of hydroxybutyl vinyl ether, 250 g of cyclohexyl dimethanol divinyl ether, 200 g of ethyl vinyl ether, 50 g of allyl glycidyl ether and 600 g of tetrafluoroethylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0144] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0145] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution with a solid content of 50 wt%.
[0146] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 26980 g / mol.
[0147] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0148] Example 9
[0149] This example uses the same reaction equipment as Example 1.
[0150] First, add 1200g of solvent xylene and 5g of auxiliary agent sodium carbonate into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of hexafluoropropylene into the reactor.
[0151] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-butyl peroxypivalate as an initiator was added to the reactor. Subsequently, 150 g of hydroxybutyl vinyl ether, 250 g of cyclohexyl dimethanol divinyl ether, 200 g of ethyl vinyl ether, 50 g of allyl glycidyl ether and 600 g of hexafluoropropylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0152] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0153] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution with a solid content of 50 wt%.
[0154] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and found to be 16920 g / mol.
[0155] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0156] Example 10
[0157] This example uses the same reaction equipment as Example 1.
[0158] First, add 1200g of solvent xylene and 5g of auxiliary agent sodium carbonate into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of trifluorochloroethylene into the reactor.
[0159] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-amyl peroxide pivalate as an initiator was added to the reactor. Subsequently, 150 g of hydroxybutyl vinyl ether, 250 g of cyclohexyl dimethanol divinyl ether, 200 g of ethyl vinyl ether, 50 g of allyl glycidyl ether and 600 g of chlorotrifluoroethylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0160] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-amyl peroxide pivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0161] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution with a solid content of 50 wt%.
[0162] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 19840 g / mol.
[0163] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0164] Embodiment 11
[0165] This example uses the same reaction equipment as Example 1.
[0166] First, add 1200g of solvent xylene and 5g of auxiliary agent sodium carbonate into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of trifluorochloroethylene into the reactor.
[0167] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-butyl peroxypivalate as an initiator was added into the reactor. Subsequently, 150 g of hydroxybutyl vinyl ether, 250 g of cyclohexyl dimethanol divinyl ether, 200 g of ethyl vinyl ether, 50 g of tetrafluoroethylene glycidyl ether and 600 g of chlorotrifluoroethylene were added into the reactor synchronously at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0168] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0169] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution with a solid content of 50 wt%.
[0170] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 32190 g / mol.
[0171] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0172] Comparative Example 1
[0173] This comparative example prepares a fluorocarbon resin without a third monomer. This comparative example uses the same reaction equipment as Example 1.
[0174] First, add 1200g of solvent xylene and 5g of auxiliary agent sodium carbonate into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of trifluorochloroethylene into the reactor.
[0175] The heating device was turned on to raise the temperature of the reactor to 54°C and maintained at this temperature, and then 12 g of t-butyl peroxypivalate as an initiator was added to the reactor. Subsequently, 450 g of vinyl acetate, 150 g of hydroxybutyl vinyl ether and 600 g of chlorotrifluoroethylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0176] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0177] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution.
[0178] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 11520 g / mol.
[0179] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0180] Comparative Example 2
[0181] This comparative example prepares a fluorocarbon resin without a third monomer. This comparative example uses the same reaction equipment as Example 1.
[0182] First, add 900g of mixed solvent butyl acetate, 300g of xylene, and 5g of auxiliary agent sodium carbonate into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is then marked as qualified. Evacuate the reactor again, and then pass 150g of trifluorochloroethylene into the reactor.
[0183] The heating device was turned on to raise the temperature of the reactor to 54°C and maintained at this temperature, and then 12 g of t-butyl peroxypivalate as an initiator was added to the reactor. Subsequently, 450 g of vinyl acetate, 150 g of hydroxybutyl vinyl ether and 600 g of chlorotrifluoroethylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0184] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0185] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution.
[0186] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 14390 g / mol.
[0187] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0188] Comparative Example 3
[0189] This comparative example prepares a fluorocarbon resin without a third monomer. This comparative example uses the same reaction equipment as Example 1.
[0190] First, add 1200g of solvent xylene and 5g of auxiliary agent sodium carbonate into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of trifluorochloroethylene into the reactor.
[0191] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-butyl peroxypivalate as an initiator was added to the reactor. Subsequently, 150 g of hydroxybutyl vinyl ether, 250 g of cyclohexyl dimethanol divinyl ether, 200 g of ethyl vinyl ether and 600 g of chlorotrifluoroethylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0192] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0193] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1 to obtain a fluorocarbon resin solution.
[0194] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 17840 g / mol.
[0195] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0196] Comparative Example 4
[0197] This comparative example prepares a fluorocarbon resin without a third monomer. This comparative example uses the same reaction equipment as Example 1.
[0198] First, add 1200g of xylene solvent and 5g of sodium carbonate auxiliary agent into the reactor, and start stirring. Seal the reactor, evacuate the reactor, and then replace it with nitrogen. Repeat the evacuation-nitrogen replacement operation until the oxygen content in the reactor is less than 20ppm, which is considered qualified. Evacuate the reactor again, and then introduce 150g of tetrafluoroethylene into the reactor.
[0199] The heating device was turned on to raise the temperature of the reactor to 54° C. and maintained at this temperature, and then 12 g of tert-butyl peroxypivalate as an initiator was added to the reactor. Subsequently, 150 g of hydroxybutyl vinyl ether, 250 g of cyclohexyl dimethanol divinyl ether, 200 g of ethyl vinyl ether and 600 g of tetrafluoroethylene were added to the reactor at a uniform rate, and the addition of the above monomers was completed within 4 hours.
[0200] After the monomer addition was completed, the temperature of the reactor was raised to 75° C. and maintained at this temperature, and then 3 g of initiator tert-butyl peroxypivalate was added to the reactor. The reactor was stirred and reacted at 75° C. for 2 hours.
[0201] After the reaction is completed, the reactor is cooled, opened, and the crude product is discharged. The crude product is concentrated, filtered, and diluted using the equipment and conditions described in Example 1, and a fluorocarbon resin solid is obtained after drying.
[0202] The number average molecular weight of the fluorocarbon resin prepared in this embodiment was measured by gel permeation chromatography and was 22910 g / mol.
[0203] The fluorocarbon resin of this embodiment was prepared into a coating according to the coating formula of Example 1, and its adhesion on the substrate was tested. The test results are summarized in Table 2.
[0204] Table 2: Adhesion test results of Examples 1-11 and Comparative Examples 1-4
[0205] Comparative Example 1 Comparative Example 2 Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Adhesion MPa 4.9 5.2 8.9 9.5 10.4 11.2 10.9 13.4 Comparative Example 3 Comparative Example 4 Example 7 Example 8 Example 9 Example 10 Embodiment 11 Adhesion MPa 5.3 5.4 9.2 9.6 10.6 11.9 13.8
Claims
1. A method for preparing a fluorocarbon resin, the method comprising: in a reactor in the presence of an initiator and an organic solvent, causing a raw material including a first monomer, a second monomer and a third monomer to undergo a copolymerization reaction to produce a fluorocarbon resin; The first monomer is a C2-C12 aliphatic hydrocarbon containing at least one carbon-carbon double bond and at least one fluorine atom, and the first monomer optionally further contains one or more non-fluorine halogen atoms; the content of the first monomer is 25-65% by weight based on the total weight of the material in the reactor; The second monomer has a structure as shown in Formula I, provided that the second monomer contains at least one carbon-carbon double bond: R1-O-R2 formula I wherein R1 and R2 are each independently selected from the group consisting of C1-C12 alkyl, C2-C12 alkenyl, C3-C12 cycloalkyl, C3-C12 cycloalkenyl, C6-C16 aralkyl, C1-C12 hydroxyalkyl, C2-C12 hydroxyalkenyl, C3-C12 hydroxycycloalkyl, C3-C12 hydroxycycloalkenyl, C2-C12 fatty alkanoyl, C6-C16 aromatic alkanoyl; and the content of the second monomer is 10-30% by weight based on the total weight of the materials in the reactor; The third monomer has a structure shown in Formula II, provided that the third monomer contains at least one carbon-carbon double bond: R3-OR 4 Formula II Wherein R3 is selected from: C2-C12 alkenyl-acyl, C6-C16 aralkenyl-acyl, fluorinated C2-C12 alkenyl-acyl, fluorinated C6-C16 aralkenyl-acyl, C2-C12 alkenyl, fluorinated C2-C12 alkenyl; R4 is selected from: C1-C8 alkyl connected with at least one epoxy (C2-C5 alkyl), C3-C12 cycloalkyl connected with at least one epoxy (C2-C5 alkyl), C6-C12 aryl connected with at least one epoxy (C2-C5 alkyl); based on the total weight of the material in the reactor, the content of the third monomer is 0.1-10 weight%.
2. The method according to claim 1, characterized in that The first monomer is selected from one or more of the following: chlorotrifluoroethylene, tetrafluoroethylene, vinylidene fluoride, hexafluoropropylene, 2,3,3,3-tetrafluoropropylene, octafluorobutene; The second monomer is selected from one or more of the following: hydroxyethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, hydroxypentyl vinyl ether, hydroxyhexyl vinyl ether, cyclobutyl vinyl ether, cyclohexyl vinyl ether, cyclohexyl dimethyl divinyl ether, ethyl vinyl ether, propyl vinyl ether, butyl vinyl ether, pentyl vinyl ether, allyl vinyl ether, vinyl benzoate, vinyl acetate, propionic acid vinyl ether, vinyl butyrate, vinyl valerate, vinyl hexanoate, vinyl nonanoate; The third monomer is selected from one or more of the following: glycidyl (meth)acrylate, allyl glycidyl ether, tetrafluorovinyl glycidyl ether, 2,3-epoxypropyl acrylate, and tetrafluorovinyl-2,3-epoxypropyl ether.
3. The method according to claim 1, characterized in that Based on the total weight of the materials in the reactor, the content of the first monomer is 35-55% by weight, the content of the second monomer is 15-25% by weight, and the content of the third monomer is 0.5-5% by weight.
4. The method according to claim 1, characterized in that The organic solvent is selected from one or more of the following: ethyl acetate, propyl acetate, butyl acetate, ethyl valerate, toluene, xylene, acetone, methyl ethyl ketone, propylene glycol methyl ether acetate; Based on the total weight of the materials in the reactor, the content of the organic solvent is 40-60% by weight.
5. The method according to claim 4, characterized in that The organic solvent is a mixture of ethyl acetate and methyl ethyl ketone in a weight ratio of 3:1 to 7:1, or a mixture of butyl acetate and xylene in a weight ratio of 3:1 to 7:1, or any one or a mixture in any proportion of pure xylene, pure butyl acetate, pure methyl ethyl ketone, and pure propylene glycol methyl ether acetate.
6. The method according to claim 1, characterized in that The initiator is selected from one or more of the following: tert-butyl peroxypivalate, diisopropyl peroxydicarbonate, tert-amyl peroxypivalate, 3-hydroxy-1,1-dimethylbutyl peroxyneodecanoic acid, tert-butyl peroxyneodecanoic acid; based on the total weight of the materials in the reactor, the content of the initiator is 0.01-2% by weight; During the copolymerization reaction, the reactor also contains an auxiliary agent, which is selected from one or more of the following: sodium carbonate, light stabilizer 292, zinc oxide, and magnesium oxide; based on the total weight of the materials in the reactor, the content of the auxiliary agent is 0.05-1% by weight; The copolymerization reaction temperature is 50-90° C., and the duration of the copolymerization reaction is 2-12 hours.
7. The method according to claim 1, characterized in that During the copolymerization reaction, at least a portion of at least one of the first monomer, the second monomer, and the third monomer is continuously added to the reactor.
8. A fluorocarbon resin, wherein the main chain thereof comprises a first copolymerization unit, a second copolymerization unit and a third copolymerization unit, wherein the content of the first copolymerization unit is 25-80% by weight, the content of the second copolymerization unit is 10-60% by weight, the content of the third copolymerization unit is 0.1-20% by weight, and the number average molecular weight of the fluorocarbon resin is 8000-40000 g / mol; in, The first copolymerized unit is derived from a first monomer, the first monomer is a C2-C12 aliphatic hydrocarbon containing at least one carbon-carbon double bond and at least one fluorine atom, and the first monomer optionally further contains one or more non-fluorine halogen atoms; The second copolymerized unit is derived from a second monomer having a structure shown in Formula I, provided that the second monomer contains at least one carbon-carbon double bond: R1-O-R2 formula I wherein R1 and R2 are each independently selected from the group consisting of C1-C12 alkyl, C2-C12 alkenyl, C3-C12 cycloalkyl, C3-C12 cycloalkenyl, C6-C16 aralkyl, C1-C12 hydroxyalkyl, C2-C12 hydroxyalkenyl, C3-C12 hydroxycycloalkyl, C3-C12 hydroxycycloalkenyl, C2-C12 fatty alkanoyl, C6-C16 aromatic alkanoyl; The third copolymerized unit is derived from a third monomer having a structure shown in Formula II, provided that the third monomer contains at least one carbon-carbon double bond: R3-O-R4 Formula II Wherein R3 is selected from: C2-C12 alkenyl-acyl, C2-C12 aralkenyl-acyl, fluorinated C2-C12 alkenyl-acyl, fluorinated C2-C12 aralkenyl-acyl, C2-C12 alkenyl, fluorinated C2-C12 alkenyl; R4 is selected from: C1-C8 alkyl connected with at least one epoxy (C2-C5 alkyl), C3-C12 cycloalkyl connected with at least one epoxy (C2-C5 alkyl), C6-C12 aryl connected with at least one epoxy (C2-C5 alkyl).
9. The fluorocarbon resin according to claim 8, which is prepared by the method according to any one of claims 1 to 7.
10. A coating product or an adhesive product comprising the fluorocarbon resin according to any one of claims 8 to 9.
Citation Information
Cited By
High-performance photocurable FEVE fluorocarbon resin as well as synthesis method and application thereof
CN119708323A