Silicon-containing block copolymer as well as preparation method and application thereof

The block copolymer PS-b-PDMS was synthesized by RAFT polymerization, and a roughened structural coating was constructed on the fabric surface by using steam-induced phase separation, which solved the problem of weakening the waterproofing ability of existing superhydrophobic materials and achieved high efficiency and durability Improved hydrophobic properties and fabric application performance.

CN118994593AActive Publication Date: 2024-11-22SUZHOU UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411052027.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-22
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The waterproofing ability of existing superhydrophobic materials quickly weakens under harsh environments or wear, and polydimethylsiloxane (PDMS) is insufficient when used as a coating material, which limits its use in fabric finishing applications, making it difficult to achieve long-term durability and efficient hydrophobicity. performance.

Method used

PS-b-PDMS with different silicon content was synthesized by RAFT polymerization, and a roughened structural coating was constructed on the fabric surface by steam-induced phase separation method. The chemistry of the target product was characterized by FT-IR and 1H-NMR. Structure, optimize silicon content and solvent type to improve hydrophobicity.

Benefits of technology

It achieves an efficient and durable superhydrophobic coating on the surface of the fabric, with a static water contact angle of up to 166.9 ± 0.2°, and maintains good performance in acid and alkali environments, water washing and adhesive testing, enhancing the fabric's usage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994593A_ABST
    Figure CN118994593A_ABST
Patent Text Reader

Abstract

The invention discloses a silicon-containing block copolymer as well as a preparation method and application thereof, and the silicon-containing block copolymer is prepared by taking carboxyl-terminated polystyrene and single-ended hydroxypropyl polydimethylsiloxane as raw materials; performing induced phase separation on the fabric with the polymer solution in a steam environment, and constructing a water-repellent durable coating on the surface of the fabric to obtain the water-repellent fabric. A steam induced phase separation method is adopted, by controlling technological parameters such as steam types, solvent types and the silicon content of polymers, roughened structure coatings are tried to be constructed on the surfaces of the terylene of different structures, the super-hydrophobic fabric is prepared, the hydrophobic property of the terylene can be better improved through the microsphere structure surface, the highest static water contact angle can reach 166.9 + / -0.2 degrees, and the super-hydrophobic fabric can be used as a super-hydrophobic fabric. And the finished fabric has good wearability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to advanced material technology and relates to a silicon-containing block copolymer, in particular to application of the silicon-containing block copolymer in preparing super-hydrophobic fabrics. Background Art

[0002] Superhydrophobicity can help keep the surface clean and reduce load and movement resistance in a short period of time, but durability is the biggest test of hydrophobicity. The waterproof ability may quickly weaken or even disappear after being exposed to harsh environments or wear. Polydimethylsiloxane (PDMS) is most commonly used in self-cleaning, oil-water separation, and anti-icing. The disadvantage of PDMS is that it lacks strength, so other materials are often added when it is used as a coating material, such as commonly used nanomaterials (silver nanowires, carbon nanotubes, etc.) and inorganic fillers (silicon dioxide, titanium dioxide, etc.). This defect limits its application in fabric finishing. Summary of the invention

[0003] The present invention adopts RAFT polymerization to synthesize block copolymers with different silicon contents, and uses FT-IR to 1 H-NMR was used to characterize the chemical structure of the target product. The steam-induced phase separation method was used to control process parameters such as steam type, solvent type and silicon content of the polymer, and roughened structure coatings were attempted to be constructed on the surface of polyester with different structures to prepare super-hydrophobic fabrics.

[0004] The present invention adopts the following technical scheme.

[0005] A silicon-containing block copolymer, the chemical structure of which is as follows: .

[0006] In the present invention, the silicon-containing block copolymer is PS- b -PDMS, the number average molecular weight of which is 2000-20000, preferably 3000-15000; in the silicon-containing block copolymer, the number average molecular weight of the trisulfide polystyrene segment is 1000-9000.

[0007] More preferably, in the silicon-containing block copolymer, the number average molecular weight of the polydimethylsiloxane is 30% to 70%, preferably 40% to 60%, and more preferably 50% to 60% of the number average molecular weight of the silicon-containing block copolymer.

[0008] The invention discloses a method for preparing the silicon-containing block copolymer, comprising the following steps: using carboxyl-terminated polystyrene and single-terminated hydroxypropyl polydimethylsiloxane as raw materials to prepare the silicon-containing block copolymer.

[0009] Furthermore, in imidazole compounds, such as N,NIn the presence of carbonyldiimidazole, the silicon-containing block copolymer is prepared using carboxyl-terminated polystyrene and single-terminated hydroxypropyl polydimethylsiloxane as raw materials.

[0010] In the present invention, S,S' -bis(α,α'-dimethyl-α''-acetic acid) trithiocarbonate and styrene are used as raw materials to prepare carboxyl-terminated polystyrene. Further, in the presence of an azo initiator, such as azobisisobutyronitrile, S,S' -Bis(α,α'-dimethyl-α''-acetic acid) trithiocarbonate and styrene are used as raw materials to prepare carboxyl-terminated polystyrene.

[0011] Preferably, the number average molecular weight of the carboxyl-terminated polystyrene is 1000-9000, preferably 2000-6000; the number average molecular weight of the single-terminated hydroxypropyl polydimethylsiloxane is 500-5000, preferably 1000-3000.

[0012] Preferably, the silicon-containing block copolymer is prepared by using carboxyl-terminated polystyrene and single-terminated hydroxypropyl polydimethylsiloxane as raw materials and reacting at 50-90° C. for 3-10 hours, preferably at 60-80° C. for 4-8 hours.

[0013] Preferably, S,S' -bis(α,α'-dimethyl-α''-acetic acid) trithiocarbonate and styrene are used as raw materials, and the reaction is kept at 50-90°C for 10-30h, preferably at 60-80°C for 15-25h to prepare terminal carboxyl polystyrene.

[0014] The invention discloses a water-repellent fabric and a preparation method thereof, comprising the following steps: inducing phase separation of a fabric with a polymer solution in a steam environment, constructing a water-repellent and durable coating on the fabric surface, and obtaining the water-repellent fabric; the polymer is the above silicon-containing block copolymer.

[0015] In the polymer solution of the present invention, the polymer is the above silicon-containing block copolymer PS- b -PDMS, the solvent includes THF (tetrahydrofuran) and CS2; the concentration of the polymer solution is 20 to 80 mg / mL, preferably 30 to 60 mg / mL.

[0016] In the present invention, the polymer solution is poured on the surface of the fabric to form a fabric with the polymer solution. Preferably, the ratio of the surface area of ​​the fabric to the polymer solution is 4 cm 2 ∶(10~100)μL, further, the ratio of the surface area of ​​the fabric to the polymer solution is 4 cm 2 ∶(20~80)μL, further, the ratio of the surface area of ​​the fabric to the polymer solution is 4 cm 2∶(25~50)μL; As common sense, the upper surface of the fabric is the surface that receives the polymer solution.

[0017] In the present invention, the steam includes water vapor and organic solvent vapor, and preferably, the organic solvent includes small molecule alcohol, such as ethanol. Preferably, the steam environment is a saturated steam environment.

[0018] In the present invention, the fabric is placed in a steam environment, and a polymer solution is added to the surface of the fabric to construct a water-repellent and durable coating. Preferably, the preparation of the water-repellent fabric is carried out at room temperature.

[0019] The invention discloses the application of the silicon-containing block copolymer in preparing water-repellent materials, especially in preparing water-repellent fabrics.

[0020] The present invention discloses the application of the water-repellent fabric in preparing functional fabrics; preferably, the application of the water-repellent fabric in preparing hydrophobic fabrics, UV-resistant fabrics, acid- and alkali-resistant fabrics or self-cleaning fabrics.

[0021] In the present invention, the fabric is a natural fiber fabric or a chemical fiber fabric, such as a cotton fabric, a polyester fabric, and the like.

[0022] The present invention uses the reversible addition-fragmentation chain transfer polymerization (RAFT) method to synthesize block copolymers (PS- b -PDMS) and used for finishing fabrics: by FT-IR and 1 H-NMR confirmed the chemical structure of the target product; GPC characterized the molecular weight and molecular weight distribution of different carboxyl-terminated polystyrenes, further proving the success and controllability of the polymerization. b -PDMS was finished onto four polyesters with different textures by using a vapor-induced phase separation process (VIPS). Using water vapor and ethanol vapor as atmosphere variables, the changes in the surface morphology and hydrophobicity of polyester under the conditions of solvent (THF and CS2), silicon content, and fabric texture were studied. The study showed that in a water vapor atmosphere, the polyester surface tended to form a microporous structure, but the distribution was very small; in an ethanol vapor atmosphere, more microsphere structures were formed, but they were mainly distributed in the fiber grooves. In addition, the microsphere structure surface is more conducive to improving the hydrophobicity of polyester, and its static water contact angle can reach up to 166.9 ± 0.2°, and the finished fabric has good wearing properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 For synthesis S,S' -Bis(α,α'-dimethyl-α''-acetic acid) trithiocarbonate, RAFT method for the synthesis of carboxyl-terminated polystyrene, and synthesis of PS- b -PDMS block copolymer route.

[0024] Figure 2 for S,S' -Infrared spectrum (top) and hydrogen nuclear magnetic resonance spectrum (bottom) of bis(α,α'-dimethyl-α”-acetic acid) trithiocarbonate.

[0025] Figure 3 The GPC spectra of carboxyl-terminated polystyrene synthesized with different feed ratios.

[0026] Figure 4 For carboxyl-terminated polystyrene (black line) and PS- b -Infrared spectrum of PDMS (red line).

[0027] Figure 5 For carboxyl-terminated polystyrene and PS- b -H NMR spectrum of PDMS: the black line is carboxyl-terminated polystyrene, the red line is PS- b -PDMS, * is deuterated chloroform, ** is deuterated dimethyl sulfoxide.

[0028] Figure 6 Schematic diagram of the steam-induced phase separation reaction apparatus.

[0029] Figure 7 SEM images and static water contact angles of untreated polyester surfaces: (a) polyester taffeta, (b) thick polyester, (c) combed polyester, and (d) cotton-like polyester.

[0030] Figure 8 SEM images of the comparative experiment of vacuum drying film of polyester taffeta: (a) silicon content 30%, (b) silicon content 50%, (c) silicon content 60%.

[0031] Fig. 9 With THF as solvent, PS- b -SEM images of PDMS phase separation under water vapor atmosphere: (a1-a3) polyester taffeta, (b1-b3) thick polyester, (c1-c3) combed polyester, (d1-d3) cotton-like polyester; (a1,b1,c1,d1) 30% silicon content, (a2,b2,c2,d2) 50% silicon content, (a3,b3,c3,d3) 60% silicon content.

[0032] Fig.10 With CS2 as solvent, PS- b -SEM of PDMS phase separation under water vapor atmosphere: (a1-a3) polyester taffeta, (b1-b3) thick polyester, (c1-c3) combed polyester, (d1-d3) cotton-like polyester; (a1, b1, c1, d1) 30% silicon content, (a2, b2, c2, d2) 50% silicon content, (a3, b3, c3, d3) 60% silicon content.

[0033] Fig.11 With THF as solvent, PS- b -SEM images of PDMS phase separation in ethanol vapor atmosphere: (a1-a3) polyester taffeta, (b1-b3) thick polyester, (c1-c3) combed polyester, (d1-d3) cotton-like polyester; (a1,b1,c1,d1) 30% silicon content, (a2,b2,c2,d2) 50% silicon content, (a3,b3,c3,d3) 60% silicon content.

[0034] Fig.12 With CS2 as solvent, PS- b -SEM images of phase separation of PDMS in ethanol vapor atmosphere: (a1-a3) polyester taffeta, (b1-b3) thick polyester, (c1-c3) combed polyester, (d1-d3) cotton-like polyester; (a1, b1, c1, d1) block copolymer with 30% silicon content, (a2, b2, c2, d2) with 50% silicon content, (a3, b3, c3, d3) with 60% silicon content.

[0035] Fig.13 The particle size distribution diagram of the microspheres with THF as solvent and ethanol as atmosphere: (a) is the block copolymer with a silicon content of 60% and polyester taffeta fabric, and (b) is the silicon content of 50% and combed polyester fabric.

[0036] Fig.14 Infrared spectra of combed polyester before and after treatment (a) and full XPS spectrum of combed polyester after treatment (b).

[0037] Fig.15 The contact angles of water on the surfaces of different polyesters treated with block copolymers: (a) water vapor atmosphere, solvent is THF; (b) water vapor atmosphere, solvent is CS2; (c) ethanol atmosphere, solvent is THF; (d) ethanol atmosphere, solvent is CS2.

[0038] Fig.16 Combed polyester was treated with a block copolymer containing 50% silicon in an ethanol vapor atmosphere using THF as solvent: (a) Untreated polyester was exposed to an aqueous solution; (b) Treated polyester was exposed to an aqueous solution; (c) The states of different droplets on the surface of the treated fabric.

[0039] Fig.17 Combed polyester finished with block copolymer containing 50% silicon in THF as solvent in ethanol vapor atmosphere: (a) adsorption capacity of carbon tetrachloride (heavy oil) in aqueous solution; (b) adsorption capacity of corn oil in aqueous solution.

[0040] Fig.18 These are the TG curve and DTG curve (nitrogen atmosphere) of combed polyester after ethanol vapor-induced phase separation treatment.

[0041] Fig.19 Static contact angle bar graphs of combed polyester after ethanol vapor-induced phase separation treatment: (a) adhesive resistance and (b) water washability.

[0042] Fig. 20 pH stability of combed polyester finished by ethanol vapor-induced phase separation: (a) static contact angle bar graph and (b) SEM images after acid-base immersion for 24 h.

[0043] Fig.21 These are the test results of water contact angle stability of fabrics treated with block polymer PDMS-b-PS and block polymer PS-b-PDMS. DETAILED DESCRIPTION

[0044] The reagents and raw materials involved in the present invention are existing products, and the specific preparation operations and performance tests are all conventional technologies. Weigh 1.2 g of tris(hydroxymethyl)aminomethane and dissolve it in water. The solution is controlled to pH=8.5 by dropping hydrochloric acid to prepare a 10 mMTris-HCl buffer solution. Polyester taffeta, 70 g / m 2 ; Combed polyester, 117 g / m 2 ; Cotton-like polyester, 123 g / m 2 ; Thick polyester, 182g / m 2 .

[0045] The synthesized intermediates and final polymers were tested using a Thermo Scientific Nicolet iS5 infrared spectrometer. The synthesized products were analyzed by hydrogen nuclear magnetic resonance spectroscopy using a BRUKER AVANCE NEO 400MHz nuclear magnetic resonance spectrometer. After the sample was placed in an NMR tube, deuterated reagents (deuterated chloroform and deuterated DMSO) were added to dissolve it, and tetramethylsilane (TMS) in the deuterated reagent was used as an internal standard for testing. The number average molecular weight (Mn) and molecular weight distribution (PDI) of the polymer were determined at 40°C using a Tosoh HLC-8320 size exclusion chromatography column (SEC) and a TSK GelMULTIITE HZ-N (3) 4.6×150 mm column. Tetrahydrofuran (THF) was used as the eluent at a flow rate of 0.35 mL·min -1. SEC samples were injected with a Tosoh HLC-8320 GPC plus autosampler. The molecular weight was calibrated with a narrow polydispersity PS standard. The cold field emission scanning electron microscope (SU8100) was used to characterize the sample morphology. The scanning electron microscope (EVO 18SEM) equipped with an energy dispersive X-ray spectrometer was used to obtain the element content and distribution on the fabric surface. The ThermoScientific Nexsa X-ray photoelectron spectrometer was used to test the elemental analysis of the fabric surface. The energy of the monochromatic AlKa source (MonoAlKa) was 1486.6 eV, and the working pressure in the cabin was 4.0×10 -9 Pa, the incident angle is 45°, and the binding energy of carbon in saturated hydrocarbons (284.6 eV) is used as the benchmark. The thermal properties of the fabric were analyzed using a thermogravimeter (Diamond 5700). The sample was cut into small pieces, about 5 mg was placed in a crucible, and then put into the instrument for testing. The test atmosphere was nitrogen, the temperature range was 30℃~700℃, and the heating rate was 10℃ / min.

[0046] The fully automatic micro droplet wettability tester (SDC-200S) was used to characterize the wettability of the finished fabric surface. The polyester fabric was fixed flatly on a glass slide using double-sided tape, and 5 μL of deionized water was used as the test droplet. The test was performed at any three points on the sample and the average value was taken.

[0047] The air permeability of the fabric was tested using a fully automatic air permeability tester (model: YG461G). The test method was in accordance with GB / T5453-1997 "Determination of Air Permeability of Textile Fabrics". The test pressure was 100 Pa, the test area was 20 cm², and the nozzle diameter was Φ 4. The final value was the average of 5 tests.

[0048] Fabric stiffness is expressed by testing flexural rigidity, and the test standard is GB / T18318.1-2009 "Determination of flexural properties of textiles". According to the standard of GB / T 3923.1-2013 "Tensile properties of textile fabrics", the changes in tensile fracture of polyester fabrics before and after finishing were tested on a universal material testing machine (model: INSTRON 5967). Embodiment 1

[0049] S,S' -Bis(α,α'-dimethyl-α''-acetic acid) trithiocarbonate (BDATC) Figure 1As shown. Under nitrogen protection, carbon disulfide (13.70 g, 0.18 mol), chloroform (53.75 g, 0.45 mol), acetone (26.15 g, 0.45 mol), tetrabutylammonium hydrogen sulfate (1.21 g, 3.55 mol) and 60.00 mL of petroleum ether were mixed in a 1000 mL single-necked flask, stirred at 10°C (vacuumed three times), and 50% NaOH (50.40 g, 1.26 mol) was added dropwise, and the entire dropwise addition time was about 90 min. The reaction was stirred overnight, 450 mL of water was added to dissolve the solid for washing, and then the water layer was acidified with 60.00 mL of concentrated HCL, stirred with N2 for 30 min, and the solid was thoroughly filtered and rinsed with water to obtain 12.88 g of dark yellow crude product. The crude product was dissolved in a mixture of toluene and acetone (volume ratio of 4:1), vacuum filtered and dried to obtain 10.00 g of bright yellow solid powder. S,S' -Bis(α,α'-dimethyl-α''-acetic acid) trithiocarbonate as a small molecule chain transfer agent.

[0050] Figure 2 for S,S' -Bis(α,α'-dimethyl-α''-acetic acid) trithiocarbonate hydrogen NMR spectrum and infrared spectrum. 1701.8 cm -1 The characteristic absorption peak at 1067.2 cm is the stretching vibration peak of C=O in the carboxyl group. -1 The characteristic absorption peak at 685.6 cm -1 The stretching vibration peak at a is attributed to -CS-, which indicates that the target product BDATC has been synthesized. The H NMR spectrum results show that the characteristic peak at a = 1.58 ppm is attributed to the hydrogen on the side chain methyl of the small molecule chain transfer agent BDATC, while the characteristic peak at b = 12.91 ppm is attributed to the hydrogen on the carboxyl groups at both ends of the BDATC molecule, which proves that the trithiocarbonate with carboxyl groups at both ends has been successfully synthesized.

[0051] The synthetic route of carboxyl-terminated polystyrene PS-BDATC is as follows: Figure 1As shown. Under nitrogen protection, 10.40 g of styrene (purified by vacuum distillation) and 282 mg of BDATC trithiocarbonate were added to a single-necked flask containing 5 mL of ultra-dry tetrahydrofuran, and 16.42 mg of azobisisobutyronitrile (AIBN, purified by recrystallization) was added. The reaction device was placed in a low-temperature magnetic stirrer that had been cooled in advance. The single-necked flask on the low-temperature magnetic stirrer was evacuated with a vacuum pump and nitrogen was passed through, and the reaction was repeated three times. The oil bath was heated to 70°C, and the reaction device was transferred to the oil bath and kept at this temperature for 17 h. After the reaction was completed, the polymerization was terminated by cooling immediately, and then the reaction solution was precipitated in ice anhydrous methanol. After filtration, it was vacuum dried for 6 h to obtain 6.89 g of yellow solid (PS-BDATC, Mn=3802), with a yield of 66%.

[0052] Referring to the above method, the amount of styrene was changed to 6.24 g to obtain the product PS-BDATC with Mn=2658.

[0053] Gel permeation chromatography (GPC) was used to test the molecular weight and molecular weight distribution of the carboxyl-terminated polystyrene products synthesized from monomer styrene and small molecule chain transfer agent at different feed ratios. The test results are as follows: Figure 3 As shown in Table 1. As the molar ratio of styrene monomer to small molecule chain transfer agent increases, the molecular weight of the resulting product, carboxyl-terminated polystyrene, increases accordingly. It is worth noting that when a low molar ratio is used, the molecular weight distribution of the prepared polymer is narrow and close to 1.0; when the molar ratio of the small molecule chain transfer agent is increased to 200:1 and 300:1, the molecular weight distribution of the resulting product becomes wider and increases to above 1.3. This result shows that the synthesis of carboxyl-terminated polystyrene in this paper conforms to the characteristics of RAFT active polymerization. According to the design requirements of the subsequent coupling method for synthesizing block polymers, the carboxyl-terminated polystyrene obtained by feeding at a molar ratio of 60:1 and 100:1 was selected as the carboxylation coupling component to obtain PS- b -PDMS block copolymer.

[0054] Table 1 GPC test results of carboxyl-terminated polystyrene with different feed (molar) ratios

[0055] Block copolymer PS- b -The synthetic route of PDMS is as follows Figure 1 Under nitrogen protection, 2.0 g of carboxyl-terminated polystyrene (PS-BDATC, Mn=3802) and 20 mL of anhydrous toluene were placed in a three-necked flask, and 196.2 mg of N,NCarbonyldiimidazole (CDI) was reacted at room temperature for 2 h, and then 2.1 g of single-end hydroxypropyl polydimethylsiloxane (Mn=2000) was added to the reaction system, and the temperature was raised to 70°C and kept for 6 h. After the reaction, the by-product imidazole was filtered out, the toluene was removed by vacuum rotary evaporation, and a light yellow solid (block polymer PS- b -PDMS) 3.2 g, yield 80%. In the infrared absorption curve, 1732.8 cm -1 The characteristic peak at is attributed to PS- b -C=O double bond of ester group in PDMS copolymer, 1061.9 cm -1 The absorption peak at δ = 0.10-0.50 ppm is attributed to the stretching vibration absorption peak of Si-O-Si; in H NMR, δ = 0.10-0.50 ppm is the chemical shift of hydrogen protons on the silicon methyl group, and a vibration peak appears at δ = 4.28 ppm, which is attributed to the methylene hydrogen (-CH2-OOC-) generated by the reaction of hydroxypropyl and terminal carboxyl groups, thus confirming the successful esterification reaction and the formation of block copolymers.

[0056] Figure 4 For carboxyl-terminated polystyrene and block copolymer PS- b -Infrared spectrum of PDMS. 1696.3 cm -1 The characteristic absorption peak at 3019.4 cm is the stretching vibration peak of the carboxyl C=O of carboxyl-terminated polystyrene. -1 The characteristic absorption peak of CH at 1732.8cm belongs to the benzene ring, indicating that carboxyl-terminated polystyrene is generated. After further esterification, the infrared absorption curve of the product is measured. -1 The characteristic peak at is attributed to PS- b -C=O double bond of ester group in PDMS copolymer, 1061.9 cm -1 The absorption peak at belongs to the stretching vibration absorption peak of Si-O-Si, indicating that the esterification is successful.

[0057] Hydrogen nuclear magnetic Figure 5 As shown, the black curve is carboxyl-terminated polystyrene. The chemical shifts of vinyl CH2 and CH protons in the polystyrene structure are located at δ=1.48 and 1.77 ppm, respectively. The hydrogen protons on the benzene ring are at δ=6.30~7.30 ppm, and the hydrogen protons of the carboxyl group at the end of polystyrene are at δ=12.06 ppm. The red curve is PS- b -PDMS block copolymer, where δ = 0.10 ~ 0.50 ppm is the chemical shift of hydrogen protons on the silicon methyl group, and a vibration peak appears at δ = 4.28 ppm, which is attributed to the methylene hydrogen (-CH2-OOC-) generated by the reaction of hydroxypropyl and terminal carboxyl groups, thus confirming the successful esterification reaction and the formation of block copolymers.

[0058] According to the above method, different proportions of PS- b -PDMS block copolymer, during esterification reaction, the molar amount of carboxyl and hydroxyl groups is the same; the silicon content is expressed as the proportion of PDMS segment molecular weight (Mn=2000 or 1000) in the total block molecular weight. b -PDMS (50%) is a copolymer of PS-BDATC (Mn=3802) and single-end hydroxypropyl polydimethylsiloxane PDMS (Mn=2000); PS- b -PDMS (60%) is a copolymer of PS-BDATC (Mn=2658) and single-end hydroxypropyl polydimethylsiloxane PDMS (Mn=2000); PS- b -PDMS (30%) is a copolymer of PS-BDATC (Mn=3802) and single-end hydroxypropyl polydimethylsiloxane PDMS (Mn=1000).

[0059] Figure 6 Schematic diagram of the device for preparing coatings for vapor-induced phase separation (VIPS). The finishing process of the fabric is carried out in a wide-mouth bottle with a sealed lid. A sponge holder is placed in the container. An appropriate amount of atmosphere solvent (water or anhydrous ethanol) is added to the container in advance. A rubber stopper is used to maintain the sealing of the container. The atmosphere is cultivated to reach saturated vapor pressure. A clean cover glass and fabric are placed on the sponge holder in turn, ensuring that there is a certain distance between the substrate and the liquid surface of the vapor atmosphere solvent. A block copolymer solution (called finishing solution, unless otherwise specified, the concentration is 40 mg / mL) is cast onto the fabric using a micro-syringe. When the organic solvent in the block copolymer solution is completely evaporated, the fabric is taken out, and a coating with a microstructure can be formed on the fabric surface.

[0060] Example 2 Process of preparing a "roughened" coating by steam-induced phase separation The polyester fabric was coated in a 30 mL wide-mouth bottle with a sealed lid. The process was as follows: a sponge holder was placed in the wide-mouth bottle, and the atmosphere solvent (water or anhydrous ethanol) was added to the container in advance. A rubber stopper was used to keep the container sealed. The atmosphere was cultivated in an oven at 25°C for 4 hours to reach the saturated vapor pressure. A clean cover glass (2.2×2.2 cm²) and fabric (2×2 cm²) were then placed on the sponge holder in turn, ensuring that the distance between the substrate (cover glass) and the vapor atmosphere solvent liquid surface was 1 cm. The bottle was sealed and allowed to stand for 30 minutes, and then 50 μL of polymer (PS- b -PDMS) solution (the solvent is THF or CS2) is cast onto the fabric. When the organic solvent in the polymer solution is completely evaporated, the fabric is taken out and a coating with a microstructure is formed on the surface of the fabric.

[0061] Polyester taffeta, combed polyester and cotton-like polyester were selected as finishing objects. In the water or ethanol vapor induced phase separation, by changing the silicon content of block copolymer, solvent type and fabric structure type, the microstructure was formed on the fabric surface according to the steam induced phase separation process, and its surface wetting properties were studied.

[0062] Comparison Example The surface morphologies of four fabrics, polyester taffeta, thick polyester, combed polyester and imitation cotton polyester, were tested (e.g. Figure 7 ), the untreated polyester fabric is obviously made of many fibers directly woven flat. The four fabrics have obvious differences in fabric feel, weaving structure, thickness and density, and also have different wettability to water.

[0063] In order to compare the morphology and performance changes of fabric finishing by steam-induced phase separation process, the fabric was directly coated with finishing liquid and dried. It was found that the surface of the fabric was completely covered with polymer film after finishing ( Figure 8 ), the hydrophobic properties of the finished fabric remain basically unchanged. Embodiment 3

[0064] In a water vapor atmosphere, the conditions for the formation of microstructure on the fabric surface by the steam-induced phase separation process and its surface wetting properties were studied by changing the silicon content of the block copolymer, the type of solvent and the type of fabric structure.

[0065] Under the condition of water vapor induced phase separation, the finishing liquid was prepared with THF as solvent, and the surface morphology of the fabric obtained by coating finishing was as follows Fig. 9 As shown. The surface of untreated polyester is smooth, and the polyester fabric treated with water vapor induced phase separation (VIPS) generates disordered porous microstructures between fibers by the finishing agent. When the percentage of silicon content in the block copolymer increases to 60%, the film coherence of the block copolymer increases and the porous substances between the fibers on the surface of the fabric increase; different polyester fabrics also behave differently, among which polyester taffeta and combed polyester form a small amount of porous film on the fiber surface when treated, while thick polyester and cotton-like polyester are covered with a smooth film.

[0066] The water vapor induced phase separation method can generate a porous film layer on a flat substrate, while the fabrics treated in this way only form a small amount of pores in the film layer. The reason is that the fabric substrate has a complex surface shape with interlaced fibers, the substrate surface is no longer flat, and the fiber material has a capillary effect on the treatment liquid, which makes the steam induced phase separation process and results different. Adjusting the treatment liquid concentration, 5 mg / mL~30 mg / mL polymer treatment liquid cannot form a good film on the fabric; 40 mg / mL finishing liquid concentration forms a good film on the fiber surface; when the treatment liquid concentration is further increased to above 60 mg / mL, a film layer can be formed to cover the fiber, but the film cracks.

[0067] Keeping other conditions unchanged, the solvent was changed to CS2, and the four fabrics were treated by water vapor induced phase separation. The surface of the obtained fabrics was as follows Fig.10 When CS2 is used as the solvent, the polymer accumulation on the surface of the treated fabric is more obvious, which is not conducive to the formation of microporous morphology in the membrane layer. Embodiment 4

[0068] The steam type was changed to ethanol, and the microstructure changes formed on the surface of the finished fabric and its surface wetting properties were studied by adjusting factors such as the silicon content of the block copolymer, the solvent type and different fabric structures.

[0069] Using ethanol as the vapor atmosphere, three types of block copolymers containing silicon, PS- b -PDMS was used to treat four polyester fabrics. The concentration of the treatment solution was 40 mg / mL and the solvent was THF. The surface morphology of the fabrics thus prepared is shown in Fig.11 When the silicon content is 30%, the treatment agent forms microspheres on the fabric surface, but the microspheres mostly grow in the gaps between the fibers.

[0070] Different fabric structures also produce differences. For example, when polyester taffeta fabric is treated with block polymers with silicon content of 30% and 50%, a small amount of microspheres are generated on the fiber surface, while when the block polymer contains 60% silicon, uniformly distributed microspheres grow on the fiber surface; when thick polyester is used as the substrate, the fabric finished with block polymer containing 30% silicon only generates a small amount of microspheres in the gaps between fibers, and when the block copolymer contains 50% silicon, the tendency of the treatment agent to separate increases, and the resulting finished thick polyester fabric is covered with a uniform spherical coating on the fiber surface. It is worth pointing out that these spherical particles are embedded in the film layer on the fiber surface, which is consistent with the characteristics of the thick polyester surface being rough and easy to adsorb and absorb the treatment agent to form a film.

[0071] When combed polyester and cotton-like polyester are treated, evenly distributed microsphere particles are formed on the surface of the fabric after finishing with a block copolymer containing 50% silicon. Among them, the surface of combed polyester is the smoothest, and when it is finished with a block copolymer containing 50% silicon, the microspheres on the fiber surface are evenly distributed and closely arranged.

[0072] When the silicon content of the block copolymer is further increased to 60%, except for polyester taffeta, the spherical particles of the other three polyesters squeeze and merge with each other after finishing, and finally form the characteristic morphology of hill-like undulating film-coated fibers, and the microspheres are no longer dispersed. When the polysiloxane chain segment accounts for a large proportion in the block copolymer, the low glass transition temperature it provides causes the block copolymer to soften, and the polymer is more likely to form a film coating on the fiber surface.

[0073] Keeping other conditions unchanged, the solvent was changed to CS2, and the block copolymer was phase-separated by ethanol vapor to finish the surfaces of the four fabrics. The surface morphology of the obtained fabrics is shown in Fig.12 As shown. Different from the polymer microphase separation and molecular chain curling into balls when the THF solution is treated in ethanol vapor, the block polymer condensed from CS2 on the fabric surface forms a more film-like coating, and the surface spherical particles decrease or even disappear. A large amount of treatment liquid stays in the fiber gaps, and spherical particles are generated by the microphase separation of the block polymer; while less treatment liquid stays on the fiber surface, and only a thin film coating is generated.

[0074] The particle size of the microsphere coating on the surface of the finished fabric was statistically analyzed. Fig.13 As shown. Among them, when the polyester taffeta fabric was treated with a block polymer THF solution containing 60% silicon, and the steam atmosphere was ethanol, the average size of the obtained microspheres was 2.90 ± 0.64 μm, and the particle distribution was uniform; for combed polyester, the treatment effect of the block polymer with a silicon content of 50% was good, and the average size of the surface microspheres in the obtained coating was 5.87 ± 1.71 μm, the particle size became larger, and the particle size distribution became wider.

[0075] ATR-FTIR and XPS were used to conduct chemical analysis on the surface of the finished fabric. Combed polyester finished in an ethanol vapor atmosphere with THF as solvent was selected for testing. The silicon content was 50%. The ATR-FTIR spectra of combed polyester before and after finishing are shown in Figure 2. Fig.14 As shown in a. Compared with the untreated combed polyester, the combed polyester treated with block copolymer coating has a -1 A new broad peak appeared at 1710.6 cm, which was attributed to the Si-O-Si stretching vibration absorption peak in the microsphere surface structure; -1 The strong C=O absorption peak at the end of the treatment weakened after finishing, which indicates that the surface of the combed polyester was PS- b -PDMS block copolymer microspheres coated. In addition, 1260.4 cm -1 The peak at 799.8 cm -1 The strong peak is attributed to the Si-(CH3)2 stretching vibration absorption peak in the block copolymer PDMS segment. Fig.14As shown in b, C, O, Si and S elements appear in the XPS spectrum of combed polyester after finishing. The presence of S element is due to the sulfur content of the small molecule chain transfer agent. Five chemical environment carbon elements, C-Si (283.93 eV), CC / CH (284.80 eV), CO (286.13 eV), C=O (288.63 eV) and C=C (282.43 eV), appear in the C 1s narrow scan spectrum. The O 1s narrow scan spectrum proves the existence of Si-O-Si (532.13 eV), C=O (533.23 eV) and CO (531.43 eV), while the Si 2p narrow scan spectrum fitting shows two peaks, which are attributed to Si-O-Si (102.08 eV) and Si-C (101.48 eV). Embodiment 5

[0076] Fig.15 The static water contact angle of the surface of polyester fabric treated by steam-induced phase separation is shown. The test found that the fabric treated with a polymer containing 30% silicon did not improve its hydrophobicity. However, the fabric treated with a block copolymer containing 50% silicon showed better hydrophobicity when phase separation was induced in a water vapor atmosphere with THF as solvent ( Fig.15 a). Among them, the contact angle of combed polyester to water after treatment reaches 151.0 ± 1.2°. When the fabric is treated with CS2 as solvent, the hydrophobicity of the treated fabric gradually increases with the increase of silicon content in the polymer ( Fig.15 b). Among them, combed polyester treated with block copolymer coatings with two silicon contents of 50% and 60% can achieve superhydrophobic effect, and the water contact angles are measured to be 157.5 ± 1.1° and 150.5 ± 0.9° respectively.

[0077] When phase separation is induced in an ethanol vapor atmosphere, Fig.15 It can be seen from Figure c that when THF is used as the solvent, the two block copolymers have better hydrophobicity. The contact angles of combed polyester after finishing are 166.9 ± 0.2° and 152.6 ± 0.6° respectively, and the contact angle of cotton-like polyester after finishing with a polymer containing 50% silicon is also 160.2 ± 0.2°. Compared with THF, when CS2 is used as the solvent for the treatment liquid, Fig.15 It can be seen from the figure d that the hydrophobicity of the treated fabric is poorly improved. The study also found that for combed polyester and cotton-like polyester, super-hydrophobicity can be achieved under this finishing condition. This is related to the fact that when the two structures of fabric are finished, a more independent and complete spherical coating is generated on the surface. It can be seen that the morphology of the coating on the surface of the fabric has a great influence on the hydrophobicity of the treated fabric.

[0078] The wettability of the finished fabric to water and other liquids was tested. Fig.16 As shown in a and b). The original polyester fabric sinks quickly when immersed in rhodamine B dyed water, while the combed polyester fabric floats on the surface of the liquid. Due to the strong capillary effect provided by the fiber structure of the untreated fabric, water droplets can easily infiltrate and diffuse into the fabric fibers; after the combed polyester is treated, the surface is super hydrophobic, so water does not infiltrate and is difficult to diffuse into the fabric fibers. Fig.16 As shown in c, the fabric has excellent repellency to liquids such as water, acid, alkali, tea and milk.

[0079] The adsorption of oil components in the water phase by the treated fabric was tested. The treated fabric was immersed in water with carbon tetrachloride oil droplets (Oil Red O dyed red) at the bottom. The carbon tetrachloride droplets were completely absorbed within a few seconds, leaving transparent water ( Fig.17 Similarly, Fig.17 In Figure b, two drops of corn oil dyed with Oil Red O were added to the water, and then the finished fabric was brought into contact with the edge of the oil droplets. The corn oil was completely absorbed by the fabric at the moment of contact. This shows that the superhydrophobic polyester fabric has good oil absorption and water repellency. Embodiment 6

[0080] The thermal stability of the fabric before and after finishing was characterized by thermogravimetric analysis. Fig.18 As shown in the figure, combed polyester is finished with a block polymer containing 50% silicon using THF as solvent. In the thermogravimetric curve, the main thermal decomposition range of the original polyester is 370℃~480℃; while the thermal decomposition range of the finished polyester moves toward the low temperature direction as a whole, between 280℃~440℃. This shows that the block polymer is finished to the surface of the fabric and decomposes earlier than the fiber matrix when heated at high temperature, resulting in mass loss. When the finished fabric is heated to 700℃, the mass residual rates are 0.43% and 12.85% respectively. Obviously, the residual mass rate of the finished fabric is greatly increased, because the silicone component in the finishing agent generates inorganic oxide residues such as SiO2 under high temperature heating conditions. Embodiment 7

[0081] Washing resistance test: The finished polyester fabric was treated with a washing fastness tester (model: WASHTEC-P), where the detergent formula was: bath ratio 1:30, neutral detergent concentration 2 g / L. The test conditions were temperature 40°C, time 30 min, and deionized water cleaning for 1 min after washing. Adhesion resistance test: 3M high-quality transparent tape was used to test the adhesion resistance of the fabric. The finished polyester fabric was pasted on a glass slide, and transparent tape was flatly pasted on the fabric. Then the tape was slowly torn off from left to right, and then torn off from right to left in the same way. This process was regarded as one cycle, and the number of cycles and the corresponding contact angle changes were recorded.

[0082] The durability of the coating on the fabric surface was tested. After washing and gluing, the coating durability was evaluated by testing the change in the static water contact angle on the fabric surface. The test results are as follows: Fig.19 As shown, (a) adhesion resistance, (b) water washing resistance; combed polyester is finished with a block polymer containing 50% silicon using THF as solvent.

[0083] Block copolymer PS- b The chemical resistance of the fabric finished with -PDMS microsphere coating was characterized by immersing the polyester fabric sample in a solution of pH = 3 or pH = 13 for 24 h (the acid was prepared by HCl and the base was prepared by NaOH), taking it out and washing and drying it, and observing the changes in SEM surface morphology and WCA. The stability of the finished combed polyester to different pH was tested. The pH = 1-14 aqueous solution was selected as the test liquid, and the static contact angle of the fabric to the aqueous solution of different pH was tested. The results are shown in Fig. 20 As shown in a. As can be seen from the figure, the finished fabric has a certain stability to acidic and alkaline aqueous solutions (pH = 3-11). In order to further explore the stability of the coating in acidic and alkaline solutions, the finished fabric was immersed in aqueous solutions of pH = 3 and pH = 13 for 24 h, respectively. The results are shown in Fig. 20 Middle b: Combed polyester finished with block polymer containing 50% silicon using THF as solvent. Example 8 Testing of Wearability of Polyester Fabric Finished with Coating by Steam-Induced Phase Separation

[0084] The wearing performance of the finished combed polyester was evaluated by breaking strength, bending stiffness and air permeability tests; ethanol was used as steam, THF was used as solvent, and the block polymer containing 50% silicon was used to finish the combed polyester. As shown in Table 2, the breaking strength and breaking elongation of the original combed polyester fabric were 257.64 N and 18.29%, respectively, and the breaking strength and breaking elongation of the finished fabric were 287.1 N and 21.19%, respectively. The breaking strength and breaking elongation of the treated combed polyester increased to a certain extent. The bending stiffness of the original combed polyester was 0.32 mN·cm, and the bending stiffness increased to 1.18 mN·cm after finishing. The air permeability of the combed polyester before and after finishing was 257.04 mm·s -1 and 268.22 mm·s -1 , the air permeability is improved, and the finished fabric still retains the inherent softness of the textile. It can be seen that the coating treatment using the steam induced phase separation process can improve the wearing performance of the fabric.

[0085] Table 2 Comparison of physical properties of untreated polyester and coated combed polyester

[0086] Comparative Example In a 10℃ water bath and nitrogen protection, add 20.19 g dodecanethiol, 48.10 g acetone, and 1.29 g tetrabutylammonium bromide to a four-necked flask in sequence. Add 50% NaOH solution (8.40 g) dropwise while stirring for no less than 20 min. Keep for 15 min after the addition, then slowly add a mixed solution of CS2 (7.61 g) and acetone (10.09 g) dropwise into the flask for no less than 20 min. The color of the solution changes from orange-yellow to wine red. Then add 17.81 g chloroform, add 50% NaOH solution (40.00 g, the addition time exceeds 30 min), and stir overnight. After that, 150 mL of distilled water was added to the four-necked flask, and then 25 mL of concentrated hydrochloric acid was added for acidification. After stirring for 30 min, a large amount of nitrogen was introduced and stirred. Finally, the filtered solid was dissolved in 250 mL of isopropanol to remove the insoluble matter. The filtrate was concentrated by rotary evaporation at 45°C, and finally the product was recrystallized with n-hexane. After drying, 20.60 g of light yellow small molecule chain transfer agent DDMAT was obtained.

[0087] Under nitrogen protection, 10.40 g of styrene (purified by vacuum distillation) and 0.47 g of DDMAT trithiocarbonate were added to a single-necked flask containing 5 mL of ultra-dry tetrahydrofuran, and 27.37 mg of azobisisobutyronitrile (AIBN, purified by recrystallization) were added. The reaction device was placed in a low-temperature magnetic stirrer that had been cooled in advance. The single-necked flask on the low-temperature magnetic stirrer was evacuated with a vacuum pump and nitrogen was passed through, and the reaction was repeated three times. The oil bath was heated to 70°C, and the reaction device was transferred to the oil bath and kept at this temperature for 17 h. After the reaction was completed, the polymerization was terminated by cooling immediately, and then the reaction solution was precipitated in ice anhydrous methanol, filtered, and vacuum dried for 6 h to obtain 6.23 g of yellow solid (PS-DDMAT), with a yield of 60%.

[0088] Under nitrogen protection, 2.00 g of carboxyl-terminated polystyrene (PS-DDMAT, Mn=3428) and 20 mL of anhydrous toluene were placed in a three-necked flask, and 94.6 mg of N,N Carbonyldiimidazole (CDI) was reacted at room temperature for 2 h, and then 1.46 g of double-terminal hydroxypropyl polydimethylsiloxane (Mn=5000) was added to the reaction system, and the temperature was raised to 70°C and kept for 6 h. After the reaction, the by-product imidazole was filtered out, the toluene was removed by vacuum rotary evaporation, and 2.98 g of yellow solid (block polymer PDMS- b -PS), yield 86%.

[0089]

[0090]

[0091] Referring to Example 1, carboxyl-terminated polystyrene (PS-BDATC, Mn=2658) and single-terminated hydroxypropyl polydimethylsiloxane (Mn=1000) were reacted to obtain PS- b -PDMS block polymer.

[0092] Steam-induced combing of polyester was carried out according to the method of Example 3, THF was used as solvent under ethanol vapor-induced phase separation, and the concentration of the polymer solution was 40 mg / mL. Block polymer PDMS- b -PS, block polymer PS- b - Water contact angle test of fabrics treated with PDMS, photos after 15 minutes of standing, see Fig.21 , the block polymer PS- b -The fabric treated with PDMS has good hydrophobic stability.

[0093] Summarize: The present invention synthesized carboxyl-terminated polystyrene with different molecular weights (number average molecular weights were 2658 and 3802, respectively) by RAFT polymerization. N,N -Carbonyldiimidazole (CDI) was used as an esterification activator and esterified with single-end hydroxypropyl PDMS (number average molecular weight of 1000 and 2000, respectively) to synthesize three block copolymers with different silicon contents: PS- b -PDMS. Using FT-IR, 1 The structure of the target product was characterized by H-NMR and GPC.

[0094] PS- b -PDMS block copolymer was used as coating treatment agent, and steam induced phase separation (VIPS) was carried out on the fabric surface (polyester taffeta, thick polyester, combed polyester and cotton-like polyester). The influence of block polymer silicon content, solvent type and other factors on the morphology was disclosed. The morphology of the coating formed on the surface was observed by SEM, and the surface wettability change was tested by contact angle meter. The results showed that in water vapor induced phase separation, a porous coating can be obtained on the fabric surface when CS2 is the solvent, among which combed polyester can obtain a hydrophobic effect after coating, and the static contact angle of water can reach 157.5 ± 1.1°, but the durability is not strong, and it is observed that water droplets wet the fabric quickly; in ethanol vapor induced phase separation, a microsphere coating can be obtained on the fabric surface when THF is the solvent. The static contact angle of the fabric to water before and after treatment was tested. The results showed that the contact angle of combed polyester under the conditions of THF solvent and 50% silicon content can reach 166.9 ± 0.2°, which has super hydrophobicity and oil absorption capacity.

[0095] The mechanical stability of the microsphere coating on the finished combed polyester was tested, and it was found that the microsphere coating could maintain a good hydrophobic effect after 6 cycles of adhesive resistance and 5 times of washing resistance tests; the finished fabric had good stability to acid and alkali. In addition, the finished polyester was still hydrophobic after 24 hours of acid and alkali immersion. Finally, the air permeability, breaking strength and bending stiffness of the finished fabric were tested, and it was found that the finished fabric had good comprehensive performance.

Claims

1. A silicon-containing block copolymer, the chemical structure of which is as follows: ; The number average molecular weight of the silicon-containing block copolymer is 2,000 to 20,000.

2. The silicon-containing block copolymer according to claim 1, characterized in that In the silicon-containing block copolymer, the number average molecular weight of the trisulfide polystyrene segment is 1000-9000.

3. The silicon-containing block copolymer according to claim 1, characterized in that: In the silicon-containing block copolymer, the number average molecular weight of the polydimethylsiloxane is 30% to 70% of the number average molecular weight of the silicon-containing block copolymer.

4. The method for preparing the silicon-containing block copolymer according to claim 1, comprising the following steps: using carboxyl-terminated polystyrene and single-terminated hydroxypropyl polydimethylsiloxane as raw materials to prepare the silicon-containing block copolymer.

5. The method for preparing the silicon-containing block copolymer according to claim 4, characterized in that: by S,S' -Bis(α,α'-dimethyl-α''-acetic acid) trithiocarbonate and styrene are used as raw materials to prepare carboxyl-terminated polystyrene.

6. A method for preparing a water-repellent fabric, comprising the following steps: inducing phase separation of a fabric with a polymer solution in a steam environment to obtain a water-repellent fabric; the polymer is the silicon-containing block copolymer according to claim 1.

7. The method for preparing a water-repellent fabric according to claim 6, characterized in that: In the polymer solution, the solvent includes THF and CS2; the concentration of the polymer solution is 20-80 mg / mL; and the steam includes water vapor and organic solvent vapor.

8. The water-repellent fabric prepared according to the method for preparing the water-repellent fabric according to claim 6.

9. Use of the silicon-containing block copolymer according to claim 1 in preparing water-repellent materials.

10. Use of the water-repellent fabric according to claim 8 in preparing functional fabrics.

Citation Information

Patent Citations

  • Amphiphilic copolymer network and preparation method thereof

    CN104592532A

  • Hydrophobic polystyrene block copolymer and preparation method thereof

    CN112142930A

  • Preparation method of homoporous membrane based on block copolymer bulk polymerization

    CN112358643A

  • Method for preparing super-hydrophobic coating through water-based RAFT miniemulsion polymerization

    CN112375450A

  • Lenses comprising amphiphilic multiblock copolymers

    US20100069522A1