Magnetic responsive water-in-water Pickering emulsion and preparation method thereof

By using the difference in solubility parameters of water-soluble polymers and mechanical stirring technology in water-soluble polymers in water-in-water Pickering emulsions, a stable magnetic responsive water-in-water Pickering emulsion was prepared, solving the problems of complex and costly preparation methods in the prior art. , the stability of the emulsion and the uniform dispersion of magnetic particles have been achieved, and the application field has been expanded.

CN118994636APending Publication Date: 2024-11-22HUAZHONG AGRI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411100927.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing magnetic responsive water-in-water Pickering emulsions are complex in preparation, the materials are expensive, and they do not conform to environmentally friendly processes. It is difficult to achieve the stability of the emulsion and the uniform dispersion of magnetic particles.

Method used

By mixing the aqueous solution of the first polymer system with the aqueous solution of the second polymer system, phase separation is performed using the difference in solubility parameters of the water-soluble polymer, particle stabilizer and hydrophilic modified magnetic particles are added to form magnetic responsiveness Water-in-water Pickering emulsion is emulsified by mechanical stirring or microfluidic emulsification to ensure uniform dispersion of magnetic particles and stability of the emulsion.

Benefits of technology

The stability of magnetically responsive water-in-water Pickering emulsion and the uniform dispersion of magnetic particles are achieved, which reduces production costs and simplifies the process flow, is suitable for laboratory and industrial production, and the behavior of the emulsion is controlled by external magnetic fields, which expands the Its application field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994636A_ABST
    Figure CN118994636A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of functional emulsion preparations, and particularly relates to a magnetic responsive water-in-water Pickering emulsion and a preparation method thereof. Mixing the aqueous solution of the first polymer system and the aqueous solution of the second polymer system, standing, and carrying out phase separation, so as to obtain two-phase aqueous solutions with different volumes; wherein the phase with smaller volume is used as a dispersed phase, and the phase with larger volume is used as a continuous phase; dispersing a particle stabilizer in the continuous phase to obtain a water-phase continuous phase in which the particle stabilizer is dispersed; dispersing hydrophilic modified magnetic particles in the dispersed phase to obtain a water-phase dispersed phase in which the magnetic particles are dispersed; and mixing the water-phase continuous phase dispersed with the particle stabilizer and the water-phase dispersed phase dispersed with the magnetic particles, and emulsifying to obtain the magnetic responsive water-in-water Pickering emulsion. By applying an external magnetic field, the behavior of the emulsion can be quickly responded and accurately controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional emulsion preparations, and more specifically, relates to a magnetically responsive water-in-water Pickering emulsion and a preparation method thereof. Background Art

[0002] Water-in-water emulsion is an immiscible dispersion system formed by mixing two or more thermally incompatible hydrophilic macromolecular aqueous solutions in a certain proportion. Water-in-water emulsion does not contain any organic solvents and surfactants, and has the advantages of safety, non-toxicity, environmental friendliness, and biocompatibility. It is widely used in food, medicine, cosmetics, packaging materials and other fields.

[0003] Water-in-water Pickering emulsions have unique interfacial characteristics and can be used as microreactors or compartmentalized operation units for the cultivation of microorganisms or cells. However, in the process of chemical reactions or biological material cultivation, it is often necessary to demulsify the Pickering emulsions with high stability at fixed times and fixed points to achieve the separation and recovery of the encapsulated materials. The use of some functional particle emulsifiers to stabilize non-invasive responsive Pickering emulsions, such as temperature response, electric field response, and ultraviolet / visible light response, can realize the functionalization of water-in-water Pickering emulsions and broaden their application areas. At present, most of the research at home and abroad is based on the construction of temperature-sensitive Pickering emulsions based on temperature-sensitive polymer materials such as poly (n-isopropylacrylamide). However, the temperature sensitivity range of the system given by this material is relatively limited, and most raw materials cannot meet the requirements of food regulations.

[0004] The water-in-water Pickering emulsion with magnetic responsiveness is an emulsion system with composite functions. The emulsion system can be used as a microcontainer in biochemical processes (such as the cultivation of microorganisms). Through the water-in-water Pickering emulsion, it is very convenient to construct a series of compartmentalized spaces that do not interfere with each other and have magnetic responsiveness, which can provide a more stable and easy-to-separate environment for the growth of microorganisms. The magnetically responsive water-in-water emulsion can be demulsified under the action of a magnetic field because the magnetic particles will aggregate under the external magnetic field, resulting in the emulsion demulsification. Specifically, when the magnetic field acts on the magnetic particles in the emulsion, they may rearrange or aggregate, resulting in the destruction of the emulsion structure, that is, the emulsifier can no longer effectively separate and stabilize the two phases. After re-stirring, the emulsifier will re-act on the two phases in the emulsion, redisperse them and form an emulsion structure. At the same time, the emulsion is guided by the external magnetic field to make the behavior of the emulsion respond quickly. The demulsification, flow, positioning, and concentration behavior of the emulsion are controlled by the synthesis and surface modification of magnetic nanoparticles, the adjustment of the emulsion preparation process, and the design of appropriate magnetic field strength and configuration. However, since the components of the water-in-water Pickering emulsion are all hydrophilic macromolecules, how to stably disperse magnetic particles in the water-in-water Pickering emulsion droplets is a challenge faced by current research. In some reports, the method for preparing a magnetic responsive emulsion is mentioned, such as the Chinese patent document application number CN112812226A discloses a magnetic responsive CPAM water-in-water emulsion and a preparation method thereof, which is prepared by passing high-purity nitrogen (N2) through acrylamide monomer, acryloyloxyethyl trimethylammonium chloride monomer, dispersant, ammonium salt, sodium salt, modified Fe3O4 nanoparticles, composite initiator and water. The formula used is complex, the material cost is high, and the characteristics of demulsification and easy recovery are not involved. Application number CN104525061A discloses a magnetically responsive Pickering emulsion based on ionic liquid and amphiphilic Fe3O4 nanoparticles, the components of which are ionic liquid and water. The ionic liquid uses uncommon salts such as 1-butyl-3-methylimidazolium hexafluorophosphate and 1-hexyl-3-methylimidazolium hexafluorophosphate, which increases the cost and is not in line with the concept of environmentally friendly process. Summary of the invention

[0005] In view of the defects of the prior art, the object of the present invention is to provide a magnetically responsive water-in-water Pickering emulsion and a preparation method thereof, and to utilize the unique structure and properties of the water-in-water Pickering emulsion to enrich its functions and broaden its application fields.

[0006] To achieve the above object, the present invention provides a method for preparing a magnetically responsive water-in-water Pickering emulsion, comprising the following steps:

[0007] (1) After the aqueous solution of the first polymer system and the aqueous solution of the second polymer system are mixed, the distribution ratio of water in the two polymer systems is different, that is, the water molecules in the polymer system with weak water retention will migrate to the polymer system with strong water retention; after standing, phase separation occurs, thereby obtaining two-phase aqueous solutions of different volumes; the smaller phase is used as the dispersed phase, and the larger phase is used as the continuous phase; the absolute value of the difference between the solubility parameter of the water-soluble polymer contained in the first polymer system relative to water and the solubility parameter of the water-soluble polymer contained in the second polymer system relative to water is greater than 0.5 (J / cm 3 ) 0.5 ;

[0008] (2) dispersing a particle stabilizer in the continuous phase to obtain an aqueous continuous phase in which the particle stabilizer is dispersed; dispersing hydrophilically modified magnetic particles in the dispersed phase to obtain an aqueous dispersed phase in which the magnetic particles are dispersed;

[0009] (3) mixing an aqueous continuous phase in which the particle stabilizer is dispersed and an aqueous dispersed phase in which the magnetic particles are dispersed, and then emulsifying the mixed phase to obtain a magnetically responsive water-in-water Pickering emulsion.

[0010] Preferably, in step (1), the first polymer system comprises one or more water-soluble polymers, and the second polymer system comprises one or more water-soluble polymers.

[0011] Preferably, the water-soluble polymer in the first polymer system and the water-soluble polymer in the second polymer system are each independently selected from synthetic macromolecules, water-soluble natural polysaccharides or water-soluble proteins.

[0012] Preferably, the mass percentage concentration of the water-soluble polymer in the aqueous solution of the first polymer system is 3.0% to 20.0%, and the mass percentage concentration of the water-soluble polymer in the aqueous solution of the second polymer system is 3.0% to 20.0%.

[0013] Preferably, the mass ratio of the aqueous solution of the first polymer system to the aqueous solution of the second polymer system is 1:1 to 1:10.

[0014] Preferably, the particle stabilizer in step (2) is water-insoluble micro-nano particles, which are one or more of inorganic nanoparticles, organic nanoparticles and inactivated microorganisms;

[0015] The mass fraction of the particle stabilizer in the aqueous continuous phase is 0.01% to 3.0%;

[0016] The inorganic nanoparticles include one or more of calcium carbonate, silicon dioxide, montmorillonite and rectorite; the organic nanoparticles include one or more of ethyl cellulose, cellulose, chitin and natural paraffin;

[0017] The particle size of the particle stabilizer is 40 to 500 nm, and the absolute value of its Zeta potential is 15 to 60 mV.

[0018] Preferably, the magnetic particles in step (3) are one or more of Fe2O3, Fe3O4, Co3O4 and NiO magnetic nanoparticles;

[0019] The particle size of the magnetic particles is 10-600 nm, more preferably 50-200 nm; the absolute value of the Zeta potential is 30-45 mV, and the mass fraction of the magnetic particles in the aqueous dispersed phase is 0.02 wt%-0.5 wt%.

[0020] Preferably, the hydrophilically modified magnetic particles are carboxyl-, sulfonic-, phosphoric- or amino-modified magnetic particles, which are obtained by introducing a hydrophilic modifier to modify the magnetic particles during the preparation process of the magnetic particles.

[0021] Further preferably, the hydrophilic modifier is a water-soluble small molecule compound or a water-soluble macromolecular substance having a carboxyl group, a sulfonic acid group, a phosphoric acid group or an amino group.

[0022] Preferably, the preparation method of the hydrophilically modified magnetic particles comprises the following steps: weighing a metal precursor of the magnetic particles, dissolving it in water and then adding the hydrophilic modifier, then adding ammonia water dropwise under heating conditions to adjust the pH to alkaline and stirring to obtain a mixed solution, and removing impurities and dehydrating the mixed solution to obtain the hydrophilically modified magnetic particles.

[0023] Preferably, in step (3), the volume ratio of the aqueous continuous phase in which the particle stabilizer is dispersed and the aqueous dispersed phase in which the magnetic particles are dispersed is (1-10):1.

[0024] Preferably, the emulsification in step (3) is mechanical stirring emulsification, membrane emulsification or microfluidic emulsification.

[0025] According to another aspect of the present invention, a magnetically responsive water-in-water Pickering emulsion prepared by the preparation method is provided.

[0026] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:

[0027] (1) Breaking through the preparation method of the traditional magnetically responsive oil-water Pickering emulsion system, the present invention constructs a magnetically responsive water-in-water Pickering emulsion system, further expanding the function of the water-in-water Pickering emulsion;

[0028] (2) In the preparation method provided by the present invention, water-soluble polymers are used as continuous phase and dispersed phase, avoiding the use of organic solvents or other toxic solvents, which can ensure high biocompatibility and low toxicity, especially in medicine, food and biological applications. The physical and chemical properties of the emulsion can be precisely adjusted according to the needs of the target application, such as adjusting the viscosity of the emulsion by changing the type and concentration of the emulsifier, using polymers of different molecular weights, and adjusting the composition of the continuous phase, adjusting the particle size of the emulsion by adjusting the emulsification technology and adjusting the emulsification parameters, and adjusting the composition of the magnetic particles and surface modification can enhance their compatibility and improve the overall stability of the emulsion.

[0029] (3) The present invention provides a magnetically responsive water-in-water Pickering emulsion and a preparation method thereof. By adding a first polymer system aqueous solution as a dispersed phase into a second polymer system aqueous solution for mixed emulsification, this method can effectively form a stable water-in-water emulsion. This efficient emulsification process helps to form uniform droplets, thereby improving the overall stability of the emulsion. In addition, this method does not require complex equipment or strict operating conditions, and only requires the use of magnetic stirring or a microporous membrane to achieve emulsification, making this method suitable for laboratory-scale research and development as well as scale-up production.

[0030] (4) The present invention provides a magnetically responsive water-in-water Pickering emulsion. The emulsion can respond quickly and be precisely controlled in its behavior (such as demulsification, flow, positioning, and concentration) by means of the guidance of an applied external magnetic field. The emulsion that has undergone demulsification or phase separation can be restored to its original stable state by magnetic stirring and can be reused multiple times, which is simple and efficient. These advantages will have broad application prospects in the fields of medicine, chemical industry, environmental science, etc.

[0031] (5) The basic formation principle of the water-in-water Pickering emulsion in the present invention is based on our previously disclosed method (CN112210087A). The difference is that the magnetically responsive water-in-water Pickering emulsion proposed in the present invention is made by embedding magnetic particles compared to other traditional magnetic emulsions. This method not only effectively increases the stability of the emulsion, but also because the magnetic particles can accurately control the structure and position of the emulsion through an external magnetic field, the magnetically responsive emulsion can achieve precise positioning or release of embedded substances. In addition, the embedded magnetic particles can be evenly dispersed in the dispersed phase of the water-in-water emulsion, reducing the risk of particle aggregation, while improving the magnetic response speed and efficiency, simplifying the production process, and improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The present invention is a flow chart of the method for preparing the magnetically responsive water-in-water Pickering emulsion.

[0033] Figure 2 This is a simulation diagram of the magnetic field-guided emulsion demulsification and phase separation of the present invention.

[0034] Figure 3 This is a diagram of the magnetic field-guided emulsion demulsification and recovery of the present invention.

[0035] Figure 4 The diagram shows the emulsion phase separation induced by an external magnetic field after adding magnetic particles of different concentrations according to the present invention.

[0036] Figure 5 is the particle size distribution of solid particles under different initial reactant concentrations.

[0037] Figure 6 This is a sample diagram of the intermediate process of preparing Fe3O4 magnetic particles using polyacrylic acid as a hydrophilic modifier.

[0038] Figure 7 Micrographs of water-in-water Pickering emulsions stabilized by Fe3O4 magnetic particles at different concentrations.

[0039] Figure 8 Micrograph of the phase separation of magnetic emulsions of Fe3O4 magnetic particles with different concentrations caused by magnets.

[0040] Fig. 9 The addition of unmodified magnetic particles did not allow for the formation of a stable emulsion by stratification under gravity. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0042] The embodiments of the present invention are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and processes are given, but the protection scope of the present invention is not limited to the following embodiments. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0043] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0044] In the present invention, unless otherwise specified and / or described, all numerical values ​​involving the amounts of components are "parts by weight" from beginning to end. The process parameters in the following examples without specifying specific conditions are usually based on conventional conditions.

[0045] In the preparation process of water-in-water Pickering emulsion, the interfacial tension of the emulsion depends on the composition of the two phases near its interface. The interfacial tension of water-in-water Pickering emulsion reaches an extremely low value near the critical point. At this time, the interfacial tension is almost zero, generally less than 10 -2 mN / m. In addition, studies at the molecular scale have found that the true thickness of this layer of water-water interface is not clear. Within a few tens of nanometers from the interface, the relative concentration of the polymer keeps changing, and the concentration is related to the displacement from the critical point. Magnetically responsive water-in-water Pickering emulsion is a functional emulsion. Because its raw materials are widely available, cheap and easy to obtain, and its behavior can be guided by artificial intervention. It has broad application prospects in the fields of drug delivery and material separation. Traditional Pickering emulsions (water-in-water, oil-in-water, water-in-oil) have defects such as complex processes or limited applications.

[0046] In view of the above problems, an embodiment of the present invention provides a method for preparing a magnetically responsive water-in-water Pickering emulsion, comprising the following steps:

[0047] (1) After the aqueous solution of the first polymer system and the aqueous solution of the second polymer system are mixed, the distribution ratio of water in the two polymer systems is different, that is, the water molecules in the polymer system with weak water retention will migrate to the polymer system with strong water retention; after standing, phase separation occurs, thereby obtaining two-phase aqueous solutions of different volumes; the smaller phase is used as the dispersed phase, and the larger phase is used as the continuous phase; the absolute value of the difference between the solubility parameter of the water-soluble polymer contained in the first polymer system relative to water and the solubility parameter of the water-soluble polymer contained in the second polymer system relative to water is greater than 0.5 (J / cm 3 ) 0.5 ;

[0048] (2) dispersing a particle stabilizer in the continuous phase to obtain an aqueous continuous phase in which the particle stabilizer is dispersed; dispersing hydrophilically modified magnetic particles in the dispersed phase to obtain an aqueous dispersed phase in which the magnetic particles are dispersed;

[0049] (3) mixing an aqueous continuous phase in which the particle stabilizer is dispersed and an aqueous dispersed phase in which the magnetic particles are dispersed, and then emulsifying the mixed phase to obtain a magnetically responsive water-in-water Pickering emulsion.

[0050] The preparation method of the water-in-water Pickering emulsion provided by the present invention is theoretically applicable to any two mutually incompatible aqueous phases that can be used to prepare the water-in-water emulsion, namely, the aqueous dispersed phase and the aqueous continuous phase. According to the Flory-Huggins polymer solution theory, the Huggins constant χ1, also known as the polymer-solvent interaction parameter, is a quantity (solvation degree) that characterizes the degree of interaction between solvent molecules and polymers, and the value is between -1 and 1, χ1<1 / 2, it is a good solvent; χ1>1 / 2 is a poor solvent. The solubility parameter is a parameter that characterizes the polymer-solvent interaction, wherein the solvent is water. The cohesive properties of a substance can be quantitatively characterized by cohesive energy, and the cohesive energy per unit volume is called cohesive energy density, and its square root is called solubility parameter. The solubility parameter can be used as a good indicator to measure whether two materials are compatible. When the solubility parameters of two materials are similar, they can be blended with each other and have good compatibility.

[0051] One of the aqueous continuous phase and the aqueous dispersed phase of the present invention is used as the solute polymer, and the other is used as the solvent. When the solubility parameters of the two are closer, the two can dissolve in each other more. The continuous phase and the dispersed phase of the present invention are aqueous solutions of two polymers, respectively. Therefore, the closer the solubility parameters of the polymers in the two aqueous solution systems used in the present invention are relative to water, the more they can dissolve in each other. The basis for preparing the water-in-water emulsion of the present invention is the continuous phase and the dispersed phase that can undergo phase separation. Therefore, according to the above-mentioned polymer solution theory, when the polymers in the two systems used in the preparation of the water-in-water Pickering emulsion of the present invention are expressed by solubility parameters, the absolute value of the difference between the solubility parameters of the polymers in the two systems relative to water is greater than 0.5. The solubility parameters of the partially water-soluble polymers used in the present invention can be obtained by looking up a table, and some can be preliminarily calculated according to theoretical parameters, or measured by conventional methods.

[0052] When preparing a water-in-water Pickering emulsion according to the present invention, the type of polymer is selected so that the absolute value of the difference between the solubility parameter of the water-soluble polymer used in the first polymer system relative to water and the solubility parameter of the water-soluble polymer used in the second polymer system relative to water is greater than 0.5, thereby obtaining an aqueous dispersed phase and an aqueous continuous phase that can undergo phase separation.

[0053] The first polymer system of the present invention comprises one or more water-soluble polymers, and the second polymer system comprises one or more water-soluble polymers, wherein the water-soluble polymers are water-soluble in a broad sense, and the water-soluble polymers include polymers that dissolve faster in water and water-swellable polymers that dissolve slower; and the absolute value of the difference in solubility parameter of the water-soluble polymers used in the first polymer system and the water-soluble polymers used in the second polymer system relative to water is greater than 0.5. When the first polymer system or the second polymer system comprises multiple polymers, the solubility parameters of the water-soluble polymers in the two systems relative to water can be determined by the sum of the products of the molar percentage of each polymer in the first polymer system or the second polymer system and the corresponding solubility parameter.

[0054] In some embodiments, in step (1), the first polymer system contains one or more water-soluble polymers, and the second polymer system contains one or more water-soluble polymers; the water-soluble polymers in the first polymer system and the water-soluble polymers in the second polymer system are each independently selected from synthetic macromolecules, water-soluble natural polysaccharides or water-soluble proteins; the mass percentage concentration of the polymer in the aqueous solution of the first polymer system is 3.0% to 20.0%, and the mass percentage concentration of the polymer in the aqueous solution of the second polymer system is 3.0% to 20.0%; the mass ratio of the aqueous solution of the second polymer system to the aqueous solution of the first polymer system is 1:1 to 1:10, preferably 1:3 to 1:5.

[0055] The water-soluble polymer described in the present invention may refer to a water-soluble macromolecule with a relative molecular mass of several thousand to several million. In some embodiments, the polymer is selected from water-soluble synthetic macromolecular polymers, water-soluble natural polysaccharides and water-soluble proteins. The water-soluble synthetic macromolecular polymers include but are not limited to polyethylene glycol, polyvinyl alcohol or polyethylene oxide, etc.; the water-soluble natural polysaccharides include but are not limited to starch, pullulan, dextran, chitosan, konjac glucomannan, dextrin, carrageenan or guar gum, etc.; the water-soluble proteins include but are not limited to gelatin, collagen or casein, etc.

[0056] In some preferred embodiments, the polymer selected in the first polymer system is one or more of dextran, hydroxypropyl methylcellulose, methylcellulose, hydroxyethyl cellulose, cold water fish skin gelatin, starch, hydroxypropyl methyl starch, hydroxyethyl starch, xanthan gum, carrageenan, guar gum, chitosan, and konjac glucomannan; the polymer selected in the second polymer system is one or more of maltodextrin, polyethylene glycol, polyethylene oxide, carrageenan, konjac glucomannan, pullulan, gelatin, collagen, and casein.

[0057] Compared with other traditional magnetic emulsions, the magnetically responsive water-in-water Pickering emulsion proposed in the present invention adopts a method of embedding magnetic particles, and a solid particle stabilizer is selected as a stabilizer.

[0058] In some embodiments, solid particle stabilizers can provide additional interface coverage to help improve the structural stability of the entire emulsion. These particles may have different surface properties and can further stabilize the emulsion through various mechanisms (such as increasing electrostatic repulsion or hydrophobic interactions between particles).

[0059] In some embodiments, the particle stabilizer in step (2) is water-insoluble micro-nanoparticles, which are one or more of inorganic nanoparticles, organic nanoparticles and inactivated microorganisms; the mass fraction of the particle stabilizer in the aqueous continuous phase is 0.01% to 3.0%; the inorganic nanoparticles include one or more of calcium carbonate, silica, montmorillonite and rectorite; the organic nanoparticles include one or more of ethyl cellulose, cellulose, chitin, natural paraffin, etc.; the particle size of the particle stabilizer is 40 to 500 nm, and the absolute value of its Zeta potential is 15 to 60 mV.

[0060] In some embodiments, the magnetic particles in step (3) are one or more magnetic nanoparticles such as Fe2O3, Fe3O4, Co3O4, NiO, etc.; the particle size of the magnetic particles is 10 to 600 nm, preferably 50-200 nm; the absolute value of its Zeta potential is 30 to 45 mV, and its mass fraction in the aqueous dispersed phase is 0.02wt% to 0.5wt%.

[0061] In some embodiments, the hydrophilically modified magnetic particles are carboxyl-, sulfonic-, phosphoric- or amino-modified magnetic particles, which are obtained by introducing a hydrophilic modifier to modify the magnetic particles during the preparation of the magnetic particles.

[0062] In some embodiments, the hydrophilic modifier is a small molecule compound or a macromolecular substance with a carboxyl group, a sulfonic acid group, a phosphoric acid group or an amino group, preferably a water-soluble macromolecular substance, such as polyacrylic acid, sodium citrate, oleic acid, and the like.

[0063] The preparation method of the magnetic particles of the present invention is different from the conventional preparation method in the prior art, except that a hydrophilic modifier is introduced during the preparation process to prepare hydrophilic modified magnetic particles. In some embodiments, the metal precursor of the magnetic particles is weighed, dissolved in water, and then the hydrophilic modifier is added, and then ammonia water is added dropwise under heating conditions to adjust the pH to alkaline and stirred, and the mixed solution is dialyzed to remove impurities, and the hydrophilic modified magnetic particles are obtained after dehydration.

[0064] In some embodiments, a trivalent iron salt, or a mixture of a trivalent iron salt and a divalent iron salt is weighed, dissolved in water, and then a hydrophilic modifier is added. Then, aqueous ammonia is added dropwise at 70-90°C to adjust the pH to 8-10, and then stirred. The mixture is reacted for 10-120 minutes to obtain a brown-red suspension or a black colloidal solution. The solution is placed in a dialysis bag and dialyzed for 12-36 hours to remove impurities, thereby obtaining an aqueous dispersion of Fe3O4 magnetic particles. Finally, the aqueous dispersion is freeze-dried to obtain black magnetic particles.

[0065] In other embodiments, a trivalent iron salt is weighed and dissolved in water, and then a hydrophilic modifier is added, and then ammonia water is added dropwise at 70-90°C to adjust the pH to 8-10, and then stirred, and reacted for 10-120 minutes to obtain a brown-red suspension; the solution is placed in a dialysis bag and dialyzed for 12-36 hours to remove impurities, and then centrifuged to obtain Fe(OH)3, and calcined at high temperature to obtain Fe2O3 magnetic particles. Fe2O3 will show certain magnetism when it is small in size, such as nanoparticle size.

[0066] Other magnetic particles can also be prepared by similar preparation methods. Dehydration treatment includes freeze drying, high temperature calcination, etc. The size of the obtained magnetic particles may be different at different treatment temperatures.

[0067] In some embodiments, the volume ratio of the aqueous continuous phase in which the particle stabilizer is dispersed and the aqueous dispersed phase in which the magnetic particles are dispersed in step (3) is (1-10):1.

[0068] In the present invention, in order to prepare a stable water-in-water Pickering emulsion, many emulsification methods in the prior art can be used, including microfluidic emulsification, microporous membrane emulsification and mechanical stirring emulsification. A preferred emulsification method, taking mechanical stirring emulsification as an example, achieves shear emulsification by the shear force generated by stirring. This method can accurately control the emulsification process, and finely regulate the size and distribution of droplets in the emulsion by adjusting the stirring speed and the feeding speed. In addition, mechanical stirring emulsification can ensure the overall stability and functionality of the emulsion. It is helpful to achieve controlled release characteristics and higher bioavailability. Mechanical stirring can be magnetic stirring, stirring paddle stirring, etc.

[0069] In some embodiments, the emulsification in step (3) is mechanical magnetic stirring emulsification, specifically: the aqueous dispersed phase is added dropwise to the aqueous continuous phase, or the aqueous dispersed phase is directly mixed with the aqueous continuous phase, and then emulsified by mechanical magnetic stirring; in a preferred embodiment, the mechanical magnetic stirring time is 15 to 30 minutes, and the stirring speed is 500 to 1000 rpm.

[0070] In some other embodiments, the emulsification in step (3) is membrane emulsification, specifically: dispersing the aqueous dispersed phase into the aqueous continuous phase through a membrane emulsification process, and the conditions of membrane emulsification are: microporous membrane pore size 1 to 20 microns, emulsification pressure: 50-900Kpa.

[0071] The magnetically responsive water-in-water Pickering emulsion prepared by the present invention can make the behavior of the emulsion (such as demulsification, flow, positioning, and concentration) respond quickly and be precisely controlled by applying an external magnetic field. The emulsion that has undergone demulsification or phase separation can be restored to its original stable state by magnetic stirring and reused multiple times, which is simple and efficient. These advantages will have broad application prospects in the fields of medicine, chemical industry, environmental science, etc.

[0072] The following are specific embodiments:

[0073] Example 1

[0074] (1) Preparation of dispersed phase and continuous phase

[0075] Weigh 20 g of xanthan gum (molecular weight 2,000,000 Da, solubility parameter 7.1 (Cal / cm 3 ) 0.5 Dissolve in 80g of deionized water to prepare a 20wt% xanthan gum aqueous solution A. Weigh 20g of dextran (molecular weight 500,000Da, solubility parameter 23.1 (Cal / cm 3 ) 0.5 Dissolve in 80g of deionized water to prepare a 20wt% dextran aqueous solution B; weigh xanthan gum aqueous solution A and dextran aqueous solution B in a solution mass ratio of 1:1, mix them, and stir them mechanically at 25°C and 2000 rpm for 30 minutes. Let them stand for phase separation, with the smaller phase as the dispersed phase and the larger phase as the continuous phase.

[0076] (2) Preparation of hydrophilically modified Fe3O4 magnetic particles

[0077] Dissolve 0.015mol of ferrous sulfate, 0.02625mol of anhydrous ferric sulfate and 0.005mol of polyacrylic acid in 100mL of distilled water and stir evenly, then add ammonia water dropwise at 80℃ to adjust pH=9 and stir, react for 30 minutes to obtain a black colloidal solution. Place the solution in a dialysis bag and dialyze for 24h to remove impurities, then freeze-dry to obtain carboxyl-modified black Fe3O4 magnetic powder. The average particle size is 120nm and the Zeta potential is -40mV.

[0078] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0079] 0.02 wt% of the carboxyl-modified Fe3O4 magnetic particles prepared in step (2) were added to the dispersed phase to obtain an aqueous dispersed phase; 0.1 wt% of nanocellulose was added to the continuous phase to obtain an aqueous continuous phase, wherein the average particle size of the nanocellulose was 200 nm and the Zeta potential was -45 mV. The two phase solutions were mixed in a volume ratio of 1:1 for aqueous dispersed phase: aqueous continuous phase, and a mechanical stirrer was used to stir for 15 min for emulsification to obtain a magnetically responsive water-in-water Pickering emulsion, wherein the average particle size of the emulsion was 4.5 μm, and no obvious phase separation phenomenon was observed after standing for 6 days. The emulsion demulsified after 50 s under the action of a neodymium iron boron magnet (BR=0.4 T), and the two phases were completely separated after 120 min. After mechanical stirring for another 10 min, a stable emulsion was re-formed.

[0080] Figure 1 Flow chart of the method for preparing magnetically responsive W / W Pickering emulsion in the examples.

[0081] Figure 2 This is a simulation diagram of magnetic field-guided emulsion demulsification and phase separation, such as Figure 2 As shown in the figure, the three stages describe the complete process from the initial emulsion state to the concentration of magnetic particles under the action of the magnetic field and finally to phase separation. The leftmost part of the figure is the emulsion obtained by dispersing small droplets in a continuous aqueous phase. The droplets are coated with magnetic nanoparticles that can respond to the external magnetic field. At the same time, the magnetic nanoparticles stabilize the dispersion of the aqueous phase droplets to prevent them from aggregating and separating. The middle part is to apply a magnetic field to the outside of the emulsion. The magnetic nanoparticles are acted upon by the magnetic force so that these magnetic nanoparticles and the water droplets coated by them are concentrated along the magnetic field lines. After the magnetic field is continuously applied in the right part, the magnetic nanoparticles and the emulsion droplets move under the guidance of the magnetic field and gradually gather on one side of the bottle to achieve the separation of the emulsion. The whole process shows the mechanism of controlling and separating the water-in-water emulsion embedded with magnetic nanoparticles using an external magnetic field.

[0082] Figure 3 This is a diagram of magnetic field-guided emulsion demulsification and recovery. Content a is the initial state when the external magnetic field is applied to the emulsion. The magnetic field has just been applied and has not yet had a significant effect on the emulsion. Content b shows that after the magnetic field is applied, the magnetic nanoparticles begin to be affected by the magnetic force and gradually move to the side close to the magnet. The magnetic nanoparticles migrate under the action of the magnetic field, and emulsion stratification begins to occur. The side close to the magnet becomes a concentrated area, while the side away from the magnet becomes clear. Content c shows that the liquid is stirred back into an emulsion state, and the magnetic nanoparticles and water droplets are redispersed throughout the liquid, making the liquid uniform again.

[0083] Figure 4The other conditions remain unchanged in Example 1, and only the concentration of the added magnetic particles is changed. The prepared emulsion is illustrated after the emulsion phase separation is guided by an external magnetic field (wherein the Fe3O4 concentration is: a: 0.01wt%; b: 0.02wt%; c: 0.05wt%; d: 0.10wt%; e: 0.2wt%). Under the action of the magnetic field, the high-concentration magnetic particles can quickly aggregate and form an obvious sedimentation layer, resulting in obvious stratification of the liquid. However, the aggregation effect of the low-concentration magnetic particles under the action of the magnetic field is not obvious, and almost no sedimentation layer is formed, and the liquid still remains relatively uniform.

[0084] Figure 5 The particle size distribution of the prepared magnetic solid particles is shown in Example 1 when other conditions remain unchanged and only the initial ferrous iron ion concentration is changed. It can be seen that when the ferrous iron salt concentration is very low, a large number of crystal nuclei are generated due to the sufficient supersaturation of the concentration for forming crystal nuclei, and the crystal nuclei growth rate is relatively low, so the resulting product particle size is relatively small. Along with the increase of the iron salt concentration, the crystal nuclei particle size increases gradually, and at this moment, the growth rate of the crystal nuclei is greater than the generation rate of the crystal nuclei, so that the particle size of the product increases.

[0085] Figure 6 This is a sample diagram of the intermediate process of preparing hydrophilic-modified Fe3O4 using polyacrylic acid as a hydrophilic modifier in Example 1; content a is before the reaction, and content b is after the reaction. The significant color change and transparency change before and after the reaction of preparing Fe3O4 magnetic particles intuitively demonstrate the successful preparation of Fe3O4 nanoparticles. The color changes from yellow or brown to black, indicating that the iron salt has been converted into Fe3O4. This significant change can be used as an important indicator to determine whether the reaction is successful.

[0086] Example 2

[0087] (1) Preparation of dispersed phase and continuous phase

[0088] Weigh 15 g of xanthan gum (molecular weight 2,000,000 Da, solubility parameter 7.1 (Cal / cm 3 ) 0.5 Dissolve in 85g of deionized water to prepare a 15wt% xanthan gum aqueous solution A. Weigh 10g of dextran (molecular weight 500,000Da, solubility parameter 23.1 (Cal / cm 3 ) 0.5 Dissolve in 90g of deionized water to prepare a 10wt% dextran aqueous solution B; weigh xanthan gum aqueous solution A and dextran aqueous solution B according to a solution mass ratio of 1:3, mix them, and stir them mechanically at 25°C and 2000 rpm for 30 minutes. Let them stand for phase separation, with the smaller phase as the dispersed phase and the larger phase as the continuous phase.

[0089] (2) Preparation of hydrophilically modified Fe3O4 magnetic particles

[0090] Dissolve 0.015mol of ferrous sulfate, 0.02625mol of anhydrous ferrous sulfate and 0.01mol of polyacrylic acid in 100mL of distilled water and stir evenly, then add ammonia water dropwise at 80℃ to adjust pH=9 and stir, react for 30 minutes to obtain a black colloidal solution. Place the solution in a dialysis bag and dialyze for 24h to remove impurities, then freeze-dry to obtain carboxyl-modified black Fe3O4 magnetic powder. The average particle size is 110nm and the Zeta potential is -47mV.

[0091] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0092] 0.06 wt% of the carboxyl-modified Fe3O4 magnetic particles prepared in step (2) were added to the dispersed phase to obtain an aqueous dispersed phase; 0.05 wt% of silica nanoparticles were added to the continuous phase to obtain an aqueous continuous phase, wherein the average particle size of the silica nanoparticles was 45 nm and the Zeta potential was -50 mV. The two phase solutions were mixed in a volume ratio of 1:3 for aqueous dispersed phase: aqueous continuous phase, and emulsified by stirring at 700 r / min for 15 min using a mechanical stirrer to obtain a magnetically responsive water-in-water Pickering emulsion, wherein the average particle size of the emulsion was 5.6 μm, and no obvious phase separation phenomenon was observed after standing for 6 days. The emulsion demulsified after 30 seconds under the action of a neodymium iron boron magnet (BR=0.4 T), and the two phases were completely separated after 100 minutes. After mechanical stirring for another 10 minutes, a stable emulsion was re-formed.

[0093] Example 3

[0094] (1) Preparation of dispersed phase and continuous phase

[0095] Weigh 12 g of xanthan gum (molecular weight 2,000,000 Da, solubility parameter 7.1 (Cal / cm 3 ) 0.5 Dissolve in 88g of deionized water to prepare a xanthan gum aqueous solution A with a mass percentage concentration of 12wt%. Weigh 5g of dextran (molecular weight 500,000Da, solubility parameter 23.1 (Cal / cm 3 ) 0.5 Dissolve in 95g of deionized water to prepare a 5wt% dextran aqueous solution B; weigh xanthan gum aqueous solution A and dextran aqueous solution B according to a solution mass ratio of 1:6, mix them, and stir them mechanically at 25°C and 2000 rpm for 30 minutes. Let them stand for phase separation, with the smaller phase as the dispersed phase and the larger phase as the continuous phase.

[0096] (2) Preparation of Fe3O4 magnetic particles

[0097] Dissolve 0.015mol of ferrous sulfate, 0.02625mol of anhydrous ferrous sulfate and 0.005mol of sodium citrate in 100mL of distilled water and stir evenly, then add ammonia water dropwise at 80℃ to adjust pH=9 and stir, react for 30 minutes to obtain a black colloidal solution. Place the solution in a dialysis bag and dialyze for 24h to remove impurities, then freeze-dry to obtain carboxyl-modified black Fe3O4 magnetic powder. The average particle size is 90nm and the Zeta potential is -43mV.

[0098] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0099] 0.10 wt% of the carboxyl-modified Fe3O4 magnetic particles prepared in step (2) were added to the dispersed phase to obtain an aqueous dispersed phase; 0.1 wt% of calcium carbonate nanoparticles were added to the continuous phase to obtain an aqueous continuous phase, the average particle size of the calcium carbonate nanoparticles was 74 nm, and the Zeta potential was -30 mV. The two phase solutions were mixed in a volume ratio of 1:6 for aqueous dispersed phase: aqueous continuous phase, and a mechanical stirrer was used to stir for 15 min for emulsification to obtain a magnetically responsive water-in-water Pickering emulsion, the average particle size of which was 6.8 μm, and no obvious phase separation phenomenon was observed after standing for 5 days. The emulsion demulsified after 25 s under the action of a neodymium iron boron magnet (BR = 0.4 T), and the two phases were completely separated after 100 min. After mechanical stirring for another 10 min, a stable emulsion was re-formed.

[0100] Example 4

[0101] (1) Preparation of dispersed phase and continuous phase

[0102] Weigh 20 g of xanthan gum (molecular weight 2,000,000 Da, solubility parameter 7.1 (Cal / cm 3 ) 0.5 Dissolve in 80g of deionized water to prepare a 20wt% xanthan gum aqueous solution A. Weigh 3g of dextran (molecular weight 500,000Da, solubility parameter 23.1 (Cal / cm 3 ) 0.5 Dissolve in 97g of deionized water to prepare a 3wt% dextran aqueous solution B; weigh xanthan gum aqueous solution A and dextran aqueous solution B at a mass ratio of 1:10, mix them, and stir them mechanically at 25°C and 2000 rpm for 30 minutes. Let them stand for phase separation, with the smaller phase as the dispersed phase and the larger phase as the continuous phase.

[0103] (2) Preparation of hydrophilically modified Fe3O4 magnetic particles

[0104] Dissolve 0.015mol of ferrous sulfate, 0.02625mol of anhydrous ferrous sulfate and 0.005mol of sodium citrate in 100mL of distilled water and stir evenly, then add ammonia water dropwise at 80℃ to adjust pH=9 and stir, react for 30 minutes to obtain a black colloidal solution. Place the solution in a dialysis bag and dialyze for 24h to remove impurities, then freeze-dry to obtain black Fe3O4 magnetic powder. The average particle size is 90nm and the Zeta potential is -43mV.

[0105] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0106] 0.20 wt% of the carboxyl-modified Fe3O4 magnetic particles prepared in step (2) were added to the dispersed phase to obtain an aqueous dispersed phase; 0.2 wt% of ethyl cellulose nanoparticles were added to the continuous phase to obtain an aqueous continuous phase, wherein the average particle size of the ethyl cellulose nanoparticles was 180 nm and the Zeta potential was -50 mV. The two phase solutions were mixed in a volume ratio of 1:10 for aqueous dispersed phase: aqueous continuous phase, and a mechanical stirrer was used to stir for 15 min for emulsification to obtain a magnetically responsive water-in-water Pickering emulsion, wherein the average particle size of the emulsion was 7.7 μm, and no obvious phase separation phenomenon was observed after standing for 5 days. The emulsion was demulsified after 20 s under the action of a neodymium iron boron magnet (BR=0.4 T), and the two phases were completely separated after 80 min. After mechanical stirring for another 10 min, a stable emulsion was re-formed.

[0107] Figure 7 The micrograph of the stable W / W Pickering emulsion obtained by changing the concentration of Fe3O4 magnetic particles in the aqueous dispersed phase while keeping other conditions unchanged, shows that the change of the emulsion droplet size within the concentration range in the figure indicates that the increase of the concentration of Fe3O4 nanoparticles will lead to a decrease in the average droplet size of the emulsion. It can be seen that Fe3O4 nanoparticles can effectively limit the coalescence of droplets in the emulsion.

[0108] Figure 8 With other conditions unchanged and only the concentration of Fe3O4 magnetic particles in the aqueous dispersed phase changed, the micrograph of the magnetic emulsion being separated by a magnet shows that, within the concentration range in the figure, the emulsion does not break obviously when a small amount of magnetic particles is added under the action of an external magnetic field, and the more magnetic particles are added, the shorter the time for the emulsion to break in the external magnetic field and the shorter the time for the emulsion to be completely stratified.

[0109] Example 5

[0110] (1) Preparation of dispersed phase and continuous phase

[0111] Weigh 15 g of hydroxypropyl methylcellulose (molecular weight 80,000 Da, solubility parameter 18.3 (Cal / cm 3 ) 0.5 Dissolve in 85g of deionized water to prepare a 15wt% hydroxypropyl methylcellulose aqueous solution A. Weigh 3g of maltodextrin (molecular weight 3,000Da, solubility parameter 25.1 (Cal / cm 3 ) 0.5 Dissolve in 97g of deionized water to prepare a 3wt% maltodextrin aqueous solution. Weigh hydroxypropyl methylcellulose aqueous solution a and maltodextrin aqueous solution B at a solution mass ratio of 1:5, and mix them by mechanical stirring at 25°C and 2000 rpm for 30 minutes. Let stand for phase separation, and take out the phase with a smaller volume as the dispersed phase and the phase with a larger volume as the continuous phase.

[0112] (2) Preparation of hydrophilically modified Fe3O4 magnetic particles

[0113] Dissolve 0.015mol of ferrous sulfate, 0.02625mol of anhydrous ferrous sulfate and 0.005mol of polyacrylic acid in 100mL of distilled water and stir evenly, then add ammonia water dropwise at 80℃ to adjust pH=9 and stir, react for 30 minutes to obtain a black colloidal solution. Place the solution in a dialysis bag and dialyze for 24h to remove impurities, then freeze-dry to obtain black Fe3O4 magnetic powder. The average particle size is 120nm and the Zeta potential is -40mV.

[0114] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0115] Add 0.1wt% of the carboxyl-modified Fe3O4 magnetic particles prepared in step (2) to the dispersed phase to obtain an aqueous dispersed phase; add 0.05wt% of silica nanoparticles to the continuous phase to obtain an aqueous continuous phase. The average particle size is 45nm and the Zeta potential is -50mV. The two-phase solution is mixed in a volume ratio of 1:5 between the aqueous dispersed phase and the aqueous continuous phase, and emulsified under an emulsification pressure of 500Kpa using a 15-micron pore size microporous membrane to obtain a magnetically responsive water-in-water Pickering emulsion. The average particle size of the emulsion is 5.6μm, and no obvious phase separation phenomenon occurs after standing for 6 days. The emulsion demulsifies after 25s under the action of a neodymium iron boron magnet (BR=0.4T), and the two phases are completely separated after 60min. After mechanical stirring for 10min, a stable emulsion is re-formed.

[0116] Example 6

[0117] (1) Preparation of dispersed phase and continuous phase

[0118] Weigh 10 g of hydroxypropyl methylcellulose (molecular weight 80,000 Da, solubility parameter 18.3 (Cal / cm 3 ) 0.5 Dissolve in 90g of deionized water to prepare a 10wt% hydroxypropyl methylcellulose aqueous solution A. Weigh 5g of maltodextrin (molecular weight 3,000Da, solubility parameter 25.1 (Cal / cm 3 ) 0.5 Dissolve in 95g of deionized water to prepare a 5wt% maltodextrin aqueous solution B. Weigh maltodextrin aqueous solution A and hydroxypropyl methylcellulose aqueous solution B in a solution mass ratio of 1:2 and mix them for 30 minutes at 25°C and 2,000 rpm by mechanical stirring. Let stand for phase separation, and take out the smaller phase as the dispersed phase and the larger phase as the continuous phase.

[0119] (2) Preparation of hydrophilically modified Fe2O3 magnetic particles

[0120] Dissolve 0.02625mol of anhydrous ferric sulfate and 0.005mol of polyacrylic acid in 100mL of distilled water and stir evenly, then add ammonia water dropwise at 80℃ to adjust pH=8 and stir, react for 60 minutes to obtain a reddish-brown suspension of Fe(OH)3. Place the solution in a dialysis bag and dialyze for 24h to remove impurities, separate the Fe(OH)3 precipitate from the solution by centrifugation and dry it, and calcine the dried Fe(OH)3 in a high-temperature furnace at 500℃ for 2h to obtain Fe2O3. The average particle size of Fe2O3 is 140nm, and the Zeta potential is -30mV.

[0121] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0122] 0.2 wt% of the carboxyl-modified Fe2O3 magnetic particles prepared in step (2) were added to the dispersed phase to obtain an aqueous dispersed phase; 0.3 wt% of nanocellulose was added to the continuous phase to obtain an aqueous continuous phase. The average particle size of the nanocellulose was 200 nm, and the Zeta potential was -45 mV. The two-phase solution was mixed in a volume ratio of 1:2 for the aqueous dispersed phase: the aqueous continuous phase, and emulsified under an emulsification pressure of 500 Kpa using a 15-micron pore size microporous membrane to obtain a magnetically responsive water-in-water Pickering emulsion. The average particle size of the emulsion was 4.9 μm, and no obvious phase separation occurred after standing for 8 days. The emulsion demulsified after 20 seconds under the action of a neodymium iron boron magnet (BR=0.4T), and the two phases were completely separated after 50 minutes. After mechanical stirring for 10 minutes, a stable emulsion was re-formed.

[0123] Example 7

[0124] (1) Preparation of dispersed phase and continuous phase

[0125] Weigh 20 g of dextran (molecular weight 500,000 Da, solubility parameter 23.1 (Cal / cm 3 ) 0.5 Dissolve in 80 g of deionized water to prepare a 20 wt% dextran aqueous solution A. Weigh 15 g of polyethylene glycol (molecular weight 88,000 Da, solubility parameter 9.38 (Cal / cm 3 ) 0.5 Dissolve 85g of deionized water to prepare a 15wt% polyethylene glycol aqueous solution B; weigh dextran aqueous solution A and polyethylene glycol aqueous solution B at a solution mass ratio of 1:5, mix them, and stir them mechanically at 25°C and 1000 rpm for 20 minutes. Let them stand for phase separation, and the phase with a smaller volume is taken as the dispersed phase, and the phase with a larger volume is taken as the continuous phase, and they are taken out separately.

[0126] (2) Preparation of Fe2O3 magnetic particles

[0127] Dissolve 0.02625mol of anhydrous ferric sulfate and 0.005mol of sodium citrate in 100mL of distilled water and mix and stir evenly, then add ammonia water dropwise at 80℃ to adjust pH=8 and stir, react for 60 minutes to obtain a reddish-brown suspension of Fe(OH)3. Place the solution in a dialysis bag and dialyze for 24h to remove impurities, separate the Fe(OH)3 precipitate from the solution by centrifugation and dry it, and calcine the dried Fe(OH)3 in a high-temperature furnace at 500℃ for 2h to obtain Fe2O3. The average particle size of Fe2O3 is 140nm, and the Zeta potential is -30mV.

[0128] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0129] 0.02 wt% of the hydrophilically modified Fe2O3 magnetic particles prepared in step (2) were added to the dispersed phase to obtain an aqueous dispersed phase; 0.1 wt% of ethyl cellulose nanoparticles were added to the continuous phase to obtain an aqueous continuous phase, the average particle size of the ethyl cellulose nanoparticles was 180 nm, and the Zeta potential was -50 mV. The two phases were mixed in a volume ratio of 1:5 for the aqueous dispersed phase: the aqueous continuous phase, and emulsified using a 15 micron pore size microporous membrane at an emulsification pressure of 500 Kpa to obtain a magnetically responsive water-in-water Pickering emulsion. The average particle size of the emulsion was 6.1 μm, and no obvious phase separation occurred after standing for 5 days. The emulsion broke down after 30 seconds under the action of a neodymium iron boron magnet (BR = 0.4 T), and the two phases were completely separated after 80 minutes. After mechanical stirring for another 12 minutes, a stable emulsion was re-formed.

[0130] Example 8

[0131] (1) Preparation of dispersed phase and continuous phase

[0132] Weigh 10 g of cold-water fish skin gelatin (molecular weight 300,000 Da, solubility parameter 23.8 (Cal / cm 3 ) 0.5 Dissolve in 40g of deionized water to prepare a 20wt% gelatin aqueous solution A; weigh 6g of dextran (molecular weight 120,000Da, solubility parameter 20.3 (Cal / cm 3 ) 0.5 Dissolve in 44g of deionized water to prepare a 12wt% dextran aqueous solution B. Weigh dextran aqueous solution A and carrageenan aqueous solution B at a solution mass ratio of 1:3, and mix them at 25°C and 2000 rpm for 30 minutes by mechanical stirring. Let stand for phase separation, and take out the smaller phase as the dispersed phase and the larger phase as the continuous phase.

[0133] (2) Preparation of hydrophilically modified Fe3O4 magnetic particles

[0134] Dissolve 0.015mol of ferrous sulfate, 0.02625mol of anhydrous ferric sulfate and 0.005mol of polyacrylic acid in 100mL of distilled water and stir evenly, then add ammonia water dropwise at 80℃ to adjust pH=9 and stir, react for 30 minutes to obtain a black colloidal solution. Place the solution in a dialysis bag and dialyze for 24h to remove impurities, then freeze-dry to obtain carboxyl-modified black Fe3O4 magnetic powder. The average particle size is 120nm and the Zeta potential is -40mV.

[0135] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0136] 0.08 wt% of the hydrophilically modified magnetic particles prepared in step (2) were added to the dispersed phase to obtain an aqueous dispersed phase; 0.1 wt% of nanocellulose was added to the continuous phase to obtain an aqueous continuous phase. The average particle size of the nanocellulose was 200 nm, and the Zeta potential was -45 mV. The two-phase solution was mixed in a volume ratio of 1:3 of aqueous dispersed phase: aqueous continuous phase, and emulsified using a 15-micron pore size microporous membrane at an emulsification pressure of 500 Kpa to obtain a magnetically responsive water-in-water Pickering emulsion. The average particle size of the emulsion was 7.6 μm, and no obvious phase separation phenomenon was observed after standing for 5 days. The emulsion demulsified after 38 seconds under the action of a neodymium iron boron magnet (BR=0.4 T), and the two phases were completely separated after 100 minutes. After mechanical stirring for 10 minutes, a stable emulsion was re-formed.

[0137] Example 9

[0138] (1) Preparation of dispersed phase and continuous phase

[0139] Weigh 10 g of konjac glucomannan (molecular weight 700,000 Da, solubility parameter 18.07 (Cal / cm 3 ) 0.5 Dissolve in 40g of deionized water to prepare a 20wt% konjac glucomannan aqueous solution A. Weigh 8g of maltodextrin (molecular weight 3,000Da, solubility parameter 25.1 (Cal / cm 3 ) 0.5 Dissolve in 40g of deionized water to prepare a 16wt% maltodextrin aqueous solution B; weigh konjac glucomannan aqueous solution A and maltodextrin aqueous solution B according to a solution mass ratio of 1:4, mix them, and stir them mechanically at 40°C and 2000 rpm for 30 minutes. Let them stand for phase separation, and the phase with a smaller volume is taken as the dispersed phase, and the phase with a larger volume is taken as the continuous phase, and they are taken out separately.

[0140] (2) Preparation of hydrophilically modified Fe3O4 magnetic particles

[0141] Dissolve 0.015mol of ferrous sulfate, 0.02625mol of anhydrous ferric sulfate and 0.005mol of polyacrylic acid in 100mL of distilled water and stir evenly, then add ammonia water dropwise at 80℃ to adjust pH=9 and stir, react for 30 minutes to obtain a black colloidal solution. Place the solution in a dialysis bag and dialyze for 24h to remove impurities, then freeze-dry to obtain carboxyl-modified black Fe3O4 magnetic powder. The average particle size is 120nm and the Zeta potential is -40mV.

[0142] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0143] 0.07 wt% of the carboxyl-modified magnetic particles prepared in step (2) were added to the dispersed phase to obtain an aqueous dispersed phase; 0.3 wt% of nanocellulose was added to the continuous phase to obtain an aqueous continuous phase. The average particle size of the nanocellulose was 200 nm and the Zeta potential was -45 mV. The two-phase solution was mixed in a volume ratio of 1:4 for the aqueous dispersed phase: the aqueous continuous phase, and emulsified using a 15-micron pore size microporous membrane at an emulsification pressure of 500 Kpa to obtain a magnetically responsive water-in-water Pickering emulsion. The average particle size of the emulsion was 6.8 μm, and no obvious phase separation occurred after standing for 5 days. The emulsion demulsified after 41 seconds under the action of a neodymium iron boron magnet (BR=0.4T), and the two phases were completely separated after 105 minutes. After mechanical stirring for 10 minutes, a stable emulsion was re-formed.

[0144] Example 10

[0145] (1) Preparation of dispersed phase and continuous phase

[0146] Weigh 20 g of dextran (molecular weight 500,000 Da, solubility parameter 23.1 (Cal / cm 3 ) 0.5 Dissolve in 30g of deionized water to prepare a 40wt% dextran aqueous solution A; weigh 5g of hydroxypropyl methylcellulose (molecular weight 80,000Da, solubility parameter 18.3 (Cal / cm 3 ) 0.5 Dissolve in 45g of deionized water to prepare a 10wt% hydroxypropyl methylcellulose aqueous solution B. Weigh konjac glucomannan aqueous solution A and maltodextrin aqueous solution B according to a solution mass ratio of 1:6, and mix them by mechanical stirring at 25°C and 2000 rpm for 30 minutes. Let stand for phase separation, and the phase with a smaller volume is used as the dispersed phase, and the phase with a larger volume is used as the continuous phase, and they are taken out separately.

[0147] (2) Preparation of hydrophilically modified Fe3O4 magnetic particles

[0148] Dissolve 0.015mol of ferrous sulfate, 0.02625mol of anhydrous ferric sulfate and 0.005mol of polyacrylic acid in 100mL of distilled water and stir evenly, then add ammonia water dropwise at 80℃ to adjust pH=9 and stir, react for 30 minutes to obtain a black colloidal solution. The solution is placed in a dialysis bag and dialyzed for 24h to remove impurities, and then freeze-dried to obtain carboxyl-modified black Fe3O4 magnetic powder. The average particle size is 150nm and the Zeta potential is -40mV.

[0149] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0150] 0.05 wt% of the carboxyl-modified magnetic particles prepared in step (2) were added to the dispersed phase to obtain an aqueous dispersed phase; 0.2 wt% of nanocellulose was added to the continuous phase to obtain an aqueous continuous phase. The average particle size of the nanocellulose was 200 nm, and the Zeta potential was -45 mV. The two-phase solution was mixed in a volume ratio of 1:6 for the aqueous dispersed phase: the aqueous continuous phase, and emulsified under an emulsification pressure of 600 Kpa using a 20-micron pore size microporous membrane to obtain a magnetically responsive water-in-water Pickering emulsion. The average particle size of the emulsion was 5.1 μm, and no obvious phase separation occurred after standing for 7 days. The emulsion broke after 43 seconds under the action of a neodymium iron boron magnet (BR=0.4T), and the two phases were completely separated after 115 minutes. After mechanical stirring for 10 minutes, a stable emulsion was re-formed.

[0151] Embodiment 11

[0152] (1) Preparation of dispersed phase and continuous phase

[0153] Weigh 20 g of dextran (molecular weight 500,000 Da, solubility parameter 23.1 (Cal / cm 3 ) 0.5 Dissolve in 80g of deionized water to prepare a 20wt% dextran aqueous solution A. Weigh 5g of maltodextrin powder (molecular weight 3,000Da, solubility parameter 25.1 (Cal / cm 3 ) 0.5 Dissolve in 95g of deionized water to prepare a 5wt% maltodextrin aqueous solution B. Weigh the glucan aqueous solution A and the maltodextrin aqueous solution B at a solution mass ratio of 1:10, and mix them at 20°C and 300 rpm for 30 minutes by mechanical stirring. Let stand for phase separation, and take out the phase with a smaller volume as the dispersed phase and the phase with a larger volume as the continuous phase.

[0154] (2) Preparation of hydrophilic modified Fe3O4 magnetic particles

[0155] Dissolve 0.015mol of ferrous sulfate, 0.02625mol of anhydrous ferric sulfate and 0.004mol of polyacrylic acid in 100mL of distilled water and stir evenly, then add ammonia water dropwise at 80℃ to adjust pH=9 and stir, react for 30 minutes to obtain a black colloidal solution. The solution is placed in a dialysis bag and dialyzed for 24h to remove impurities, and then freeze-dried to obtain carboxyl-modified black Fe3O4 magnetic powder. The average particle size is 100nm and the Zeta potential is -35mV.

[0156] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0157] 0.02 wt% of the carboxyl-modified magnetic particles prepared in step (2) were added to the dispersed phase to obtain an aqueous dispersed phase; 0.1 wt% of silica nanoparticles were added to the continuous phase to obtain an aqueous continuous phase. The average particle size was 45 nm and the Zeta potential was -50 mV. The two-phase solution was mixed in a volume ratio of 1:10 of aqueous dispersed phase: aqueous continuous phase, and emulsified using microfluidic technology to obtain a magnetically responsive water-in-water Pickering emulsion. The average particle size of the emulsion was 3.0 μm, and no obvious phase separation occurred after standing for 4 days. The emulsion was demulsified after 15 seconds under the action of a neodymium iron boron magnet (BR=0.4T), and the two phases were completely separated after 40 minutes. After mechanical stirring for 10 minutes, a stable emulsion was re-formed. This shows that under the action of an external magnetic field, the magnetic particles of the emulsion prepared in this embodiment will aggregate and precipitate from the emulsion, destroying the emulsion structure. After the external magnetic field is removed, the magnetic particles return to a dispersed state and the emulsion structure can be restored.

[0158] Comparative Example 1

[0159] Step (1) is the same as in Example 10.

[0160] (2) Preparation of Fe3O4 magnetic particles

[0161] Dissolve 0.015mol of ferrous sulfate and 0.02625mol of anhydrous ferric sulfate in 100mL of distilled water and stir evenly without adding any modifying substances. Then, add ammonia water dropwise at 80℃ to adjust the pH to 9 and stir. React for 30 minutes to obtain a black colloidal solution. Place the solution in a dialysis bag and dialyze for 24h to remove impurities, and then freeze-dry to obtain black Fe3O4 magnetic powder. The average particle size is 385nm and the Zeta potential is -26mV.

[0162] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0163] Add 0.5 wt% of the non-hydrophilically modified magnetic particles prepared in step (2) to the dispersed phase to obtain an aqueous dispersed phase; add 0.2 wt% of nanocellulose to the continuous phase to obtain an aqueous continuous phase. The average particle size of the nanocellulose is 200 nm, and the Zeta potential is -45 mV. The two phases are mixed in a volume ratio of 1:6 of aqueous dispersed phase:aqueous continuous phase, and emulsified using a 20-micron pore size microporous membrane at an emulsification pressure of 600 Kpa to obtain a water-in-water Pickering emulsion. The average particle size of the emulsion is 7.8 μm. The emulsion demulsified after standing for 12 hours, and the two phases were completely separated after 28 hours, and no stable emulsion could be formed. Fig. 9 As shown, when the magnetic particles are not hydrophilically modified, the emulsion separates under the action of gravity and cannot form a stable emulsion.

[0164] Comparative Example 2

[0165] Step (1) is the same as in Example 5.

[0166] (2) Preparation of Fe3O4 magnetic particles

[0167] Dissolve 0.015mol of ferrous sulfate and 0.02625mol of anhydrous ferric sulfate in 100mL of distilled water and stir evenly without adding any modified substances. Then, add ammonia water dropwise at 80℃ to adjust the pH to 9 and stir. React for 30 minutes to obtain a black colloidal solution. Place the solution in a dialysis bag and dialyze for 24h to remove impurities. Then, freeze-dry to obtain black Fe3O4 magnetic powder without hydrophilic modification. The average particle size is 385nm and the Zeta potential is -26mV.

[0168] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0169] Add 0.1wt% of the non-hydrophilically modified magnetic particles prepared in step (2) to the dispersed phase to obtain an aqueous dispersed phase; add 0.05wt% of silica nanoparticles to the continuous phase to obtain an aqueous continuous phase. The average particle size is 45nm and the Zeta potential is -50mV. The two phases are mixed in a volume ratio of 1:5 of aqueous dispersed phase:aqueous continuous phase, and emulsified using a 15-micron pore size microporous membrane at an emulsification pressure of 500Kpa to obtain a magnetically responsive water-in-water Pickering emulsion. The average particle size of the emulsion is 7.3μm. The emulsion demulsified after standing for 7h, and the two phases were completely separated after 24h, and a stable emulsion could not be formed.

[0170] Comparative Example 3

[0171] Step (1) is the same as in Example 6.

[0172] (2) Preparation of Fe2O3 magnetic particles

[0173] Dissolve 0.02625 mol of anhydrous ferric sulfate in 100 mL of distilled water and stir evenly without adding any modifying substances. Then, add ammonia water dropwise at 80°C to adjust the pH to 8 and stir. React for 60 minutes to obtain a reddish-brown suspension of Fe(OH)3. Place the solution in a dialysis bag and dialyze for 24 hours to remove impurities. Separate the Fe(OH)3 precipitate from the solution by centrifugation and dry it. The dried Fe(OH)3 is calcined in a high-temperature furnace at 500°C for 2 hours to obtain Fe2O3. The average particle size of Fe2O3 is 320 nm and the Zeta potential is -23 mV.

[0174] (3) Preparation of magnetically responsive water-in-water Pickering emulsion

[0175] 0.2wt% of unmodified magnetic particles were added to the dispersed phase to obtain an aqueous dispersed phase; 0.3wt% of nanocellulose was added to the continuous phase to obtain an aqueous continuous phase. The average particle size of the nanocellulose was 200nm and the Zeta potential was -45mV. The two-phase solution was mixed in a volume ratio of 1:2 of aqueous dispersed phase: aqueous continuous phase, and emulsified using a 15-micron pore size microporous membrane at an emulsification pressure of 500Kpa to obtain a magnetically responsive water-in-water Pickering emulsion. The average particle size of the emulsion was 6.8μm. The emulsion broke after standing for 12h, and the two phases were completely separated after 28h, and a stable emulsion could not be formed.

[0176] It can be seen from Comparative Examples 1 to 3 that if the hydrophilic modification is not performed when preparing the magnetic nanoparticles, the magnetic nanoparticles are directly added to the aqueous dispersed phase and coated in the emulsion, and a magnetic emulsion system cannot be formed. This may be because the magnetic particles will agglomerate to form large aggregates due to magnetic attraction and precipitate from the emulsion. This shows that in order to prepare a stable magnetically responsive water-in-water emulsion in the embodiments of the present invention, it is very important to modify the surface of the magnetic nanoparticles.

[0177] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a magnetically responsive water-in-water Pickering emulsion, It is characterized in that The steps include: (1) After the aqueous solution of the first polymer system and the aqueous solution of the second polymer system are mixed, the distribution ratio of water in the two polymer systems is different, that is, the water molecules in the polymer system with weak water retention will migrate to the polymer system with strong water retention; after standing, phase separation occurs, thereby obtaining two-phase aqueous solutions of different volumes; the smaller phase is used as the dispersed phase, and the larger phase is used as the continuous phase; the absolute value of the difference between the solubility parameter of the water-soluble polymer contained in the first polymer system relative to water and the solubility parameter of the water-soluble polymer contained in the second polymer system relative to water is greater than 0.5 (J / cm 3 ) 0.5 ; (2) dispersing a particle stabilizer in the continuous phase to obtain an aqueous continuous phase in which the particle stabilizer is dispersed; dispersing hydrophilically modified magnetic particles in the dispersed phase to obtain an aqueous dispersed phase in which the magnetic particles are dispersed; (3) mixing an aqueous continuous phase in which the particle stabilizer is dispersed and an aqueous dispersed phase in which the magnetic particles are dispersed, and then emulsifying the mixed phase to obtain a magnetically responsive water-in-water Pickering emulsion.

2. The preparation method according to claim 1, It is characterized in that Step (1) the first polymer system comprises one or more water-soluble polymers, and the second polymer system comprises one or more water-soluble polymers; and / or, The water-soluble polymer in the first polymer system and the water-soluble polymer in the second polymer system are each independently selected from synthetic macromolecules, water-soluble natural polysaccharides or water-soluble proteins; and / or, The mass percentage concentration of the water-soluble polymer in the aqueous solution of the first polymer system is 3.0% to 20.0%, and the mass percentage concentration of the water-soluble polymer in the aqueous solution of the second polymer system is 3.0% to 20.0%; The mass ratio of the aqueous solution of the first polymer system to the aqueous solution of the second polymer system is 1:1 to 1:

10.

3. The preparation method according to claim 1, It is characterized in that The particle stabilizer in step (2) is water-insoluble micro-nano particles, which are one or more of inorganic nanoparticles, organic nanoparticles and inactivated microorganisms; The mass fraction of the particle stabilizer in the aqueous continuous phase is 0.01% to 3.0%; The inorganic nanoparticles include one or more of calcium carbonate, silicon dioxide, montmorillonite and rectorite; the organic nanoparticles include one or more of ethyl cellulose, cellulose, chitin and natural paraffin; The particle size of the particle stabilizer is 40 to 500 nm, and the absolute value of its Zeta potential is 15 to 60 mV.

4. The preparation method according to claim 1, It is characterized in that The magnetic particles in step (3) are Fe 2 O 3 , Fe 3 O 4 、Co 3 O 4 and one or more of NiO magnetic nanoparticles; The particle size of the magnetic particles is 10 to 600 nm; the absolute value of the Zeta potential is 30 to 45 mV, and the mass fraction of the magnetic particles in the aqueous dispersed phase is 0.02 wt % to 0.5 wt %.

5. The preparation method according to claim 1, It is characterized in that The hydrophilically modified magnetic particles are carboxyl-, sulfonic-, phosphoric- or amino-modified magnetic particles, which are obtained by introducing a hydrophilic modifier into the magnetic particles during the preparation process to modify them.

6. The preparation method according to claim 5, It is characterized in that The hydrophilic modifier is a water-soluble small molecule compound or a water-soluble macromolecular substance with a carboxyl group, a sulfonic acid group, a phosphoric acid group or an amino group.

7. The preparation method according to claim 6, It is characterized in that The preparation method of the hydrophilically modified magnetic particles comprises the following steps: weighing a metal precursor of the magnetic particles, dissolving it in water, adding the hydrophilic modifier, then adding ammonia water dropwise under heating conditions to adjust the pH to alkaline and stirring to obtain a mixed solution, and removing impurities and dehydrating the mixed solution to obtain the hydrophilically modified magnetic particles.

8. The preparation method according to claim 1, It is characterized in that In step (3), the volume ratio of the aqueous continuous phase in which the particle stabilizer is dispersed and the aqueous dispersed phase in which the magnetic particles are dispersed is (1-10):

1.

9. The preparation method according to claim 1, It is characterized in that The emulsification in step (3) is mechanical stirring emulsification, membrane emulsification or microfluidic emulsification. 10 . The magnetically responsive water-in-water Pickering emulsion prepared by the preparation method according to claim 1 .