Epoxy siloxane-containing additive, ionizing radiation-resistant saturated aliphatic polyester material and preparation method of ionizing radiation-resistant saturated aliphatic polyester material
By adding epoxy silicone as a radiation-resistant additive to saturated aliphatic polyester materials, the problem of easy decomposition of polyester materials under high ionization radiation is solved, and the mechanical properties of high radiation doses are maintained and reduced radiation decomposition is achieved. The trend avoids radiation yellowing and toxicity problems and has good industrial application prospects.
Patent Information
- Application Number
- CN202411092849.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
Under high ionizing radiation dose, aliphatic polyester materials with saturated C-C or C-O units on the backbone are easily decomposed during radiation disinfection, resulting in a decrease in mechanical properties. The existing radiation-resistant formulas have radiation yellowing and toxicity problems.
Using epoxy silicone as radiation-resistant additives, combined with saturated aliphatic polyester materials, saturated aliphatic polyester materials with ionizing and granulation processes are prepared. The additive molecular structure does not contain aromatic hydrocarbons, is low toxicity, and has a high boiling point. , can reduce or delay radiation decomposition of the material at high radiation doses.
It significantly reduces or delays the radiation decomposition trend of saturated aliphatic polyester materials, improves its mechanical properties under high radiation doses, avoids the radiation yellowing and toxicity problems of traditional radiation-resistant agents, and has good industrial application prospects.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of radiation-resistant modification of materials, and in particular to an epoxysiloxane-containing additive, an ionizing radiation-resistant saturated aliphatic polyester material and a preparation method thereof. Background Art
[0002] At present, for environmental protection, the use of various types of degradable plastics is strongly advocated at home and abroad. Some degradable plastics have been widely used in import and export goods shells or packaging materials, disposable medical plastic products, etc. Among them, the polymer with aliphatic polyester structure (i.e., only containing saturated CC and CO chains) as the main chain is one of the mature commercialized degradable plastics, such as polybutylene succinate (PBS), polylactic acid (PLA), etc. However, this type of polyester material is often faced with the treatment process that requires radiation disinfection in the above uses. After various ionizing radiation disinfection treatments (gamma ray radiation disinfection, electron beam radiation disinfection), due to the lack of radiation-resistant groups in their molecular chain unit, they are usually very sensitive to radiation degradation. Generally, when the radiation dose reaches more than tens of kGy, it will cause obvious mechanical property degradation due to radiation degradation. Therefore, for this type of degradable polyester, it is necessary to make full use of its degradable environmental protection properties, and it is urgent to improve its ionizing radiation resistance. The research and development of radiation-resistant formulas suitable for this type of polyester material has practical needs and economic value.
[0003] Based on this, the present invention provides an anti-radiation additive formula suitable for aliphatic polyester materials whose molecular chain structure is mainly fully saturated CC or CO units, and a composite material and preparation method thereof. Summary of the invention
[0004] The present invention aims to provide a low-toxic, high-boiling-point radiation-resistant additive to address the problem of aliphatic polyester being susceptible to radiation decomposition under high ionizing radiation doses. Compared with other conventional radiation-resistant formulations, the formulation has no radiation yellowing disadvantage and can significantly reduce or delay the radiation decomposition trend of saturated aliphatic polyester materials under a radiation dose of at least 200 kGy.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0006] An additive is applicable to a formulation system of saturated aliphatic polyester for resisting ionizing radiation, and the additive contains epoxysiloxane.
[0007] As a possible implementation mode, further, the saturated aliphatic polyester is a polycarboxylate whose main chain structure is a saturated aliphatic chain structure, such as polybutylene succinate (PBS), polylactic acid (PLA), polybutylene adipate (PBA), polycaprolactone (PCL) and other aliphatic polyesters without aromatic structures.
[0008] As a possible implementation, further, the epoxysiloxane is an organic silicon compound having an epoxy group at one end of the molecular chain and an alkoxysilane structure at the other end, and the intermediate molecular structure connecting the two ends is a saturated CC or CO chain, such as: 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, etc. Any molecular structure similar to (R 1 O) 3 Si-R 2 -OR 3 -(CHOCH)-form organosilicon compounds, wherein R n represents an alkyl group, and -(CHOCH)- represents an epoxy group.
[0009] The present invention also provides a saturated aliphatic polyester material resistant to ionizing radiation, comprising the saturated aliphatic polyester and the above-mentioned additive.
[0010] As a possible implementation manner, further, the epoxysiloxane is added in an amount of 0.1% to 10% relative to the total weight of the feed.
[0011] Furthermore, the saturated aliphatic polyester material resistant to ionizing radiation does not contain aromatic structures and unsaturated olefin units; and the additive formula components can withstand processing temperatures below 300 degrees.
[0012] The present invention provides a method for preparing the above-mentioned ionizing radiation resistant saturated aliphatic polyester material, characterized in that it comprises the following steps:
[0013] 1) Pre-drying the saturated aliphatic polyester raw material for standby use;
[0014] 2) adding the epoxysiloxane type additive to the dried saturated aliphatic polyester pure raw material and stirring to mix well;
[0015] 3) adding the mixed material to a melting device such as an internal mixer or a screw extruder, and mixing it at the internal mixing temperature of the pure raw material of the saturated aliphatic polyester to be processed until it is uniform;
[0016] 4) The material after the banburying in step 3) is crushed and then re-granulated to obtain a saturated aliphatic polyester modified composite masterbatch.
[0017] As a possible implementation, further, in step 2), the epoxysiloxane is added separately to the pure saturated aliphatic polyester raw material, or the epoxysiloxane is added to the polyester raw material in batches during the mixing process of step 3).
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0019] 1) The molecular chemical structure of the additive provided by the present invention does not contain aromatic hydrocarbon groups such as benzene rings. The epoxy group has basically no residue and is non-toxic after sufficient ring-opening reaction during the banburying and irradiation process. The siloxane group is also low-toxic and harmless. In addition, the two main functional molecular groups do not have a color-producing molecular structure, which fundamentally avoids the problems of radiation yellowing and high toxicity of traditional aromatic hydrocarbon anti-radiation agents.
[0020] 2) The additive of the present invention has a high boiling point and low volatility, can reduce air pollution during the processing, and can significantly alleviate the radiation degradation trend of saturated aliphatic polyester, and has excellent industrial application prospects. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] The polyester raw material used in the following examples is polybutylene succinate (PBS), and the additive is 3-(2,3-epoxypropoxy)propyltrimethoxysilane.
[0023] The preparation method of the saturated aliphatic polyester material resistant to ionizing radiation specifically comprises the following steps:
[0024] 1) The saturated aliphatic polyester raw material is first dried in a drying equipment such as a blast dryer at 60-80°C for 1-4 hours for use. If it is not used immediately after drying, the polyester raw material is sealed in a dry state at 30-40°C. If it is stored openly, it needs to be dried again before use;
[0025] 2) Adding additives in a weight percentage relative to the total feed, wherein the epoxysiloxane is added in an amount of 0.1% to 10%; mixing the additives with the polyester pellets dried in the above step 1) and stirring evenly, the epoxysiloxane can be added separately to the pure saturated aliphatic polyester raw material, or added gradually during the subsequent mixing and kneading process.
[0026] 3) The mixture in step 2) is put into a mixing device such as an internal mixer for internal mixing. The internal mixing temperature is set to be near the melting temperature of the pure saturated aliphatic raw material. The internal mixing time is 5 to 30 minutes. During this period, the remaining additives that need to be added multiple times can be added successively.
[0027] 4) The raw materials after mixing are taken out and crushed by a plastic crusher and other equipment, and then re-granulated to obtain the final granular radiation-resistant composite material, which can be used as the masterbatch of various plastic products for anti-ionizing radiation purposes. It has good anti-ionizing radiation performance and can be used alone or blended with other plastics.
[0028] Example 1
[0029] Take 99% of polybutylene succinate (PBS) raw material (relative to the weight percentage of the total feed, the following percentages have the same meaning), dry it in a blast dryer at 60 degrees for about 2 hours, cool it down to 30-40 degrees and take it out. Mix 1% of the additive 3-(2,3-epoxypropoxy)propyltrimethoxysilane with the dried PBS masterbatch. Then put the mixture into a mixer and mix it at 140℃ for 5-8 minutes. After the mixing is completed, take it out and put it into a plastic crusher for crushing. Put the crushed mixture into a twin-screw extruder for re-granulation. The temperature of each zone of the extruder is 120-140℃ and the speed is 40-60r / min.
[0030] The radiation-resistant composite material finally obtained in this embodiment is injected into a dumbbell-shaped mechanical test sample to test the change of the formula on the radiation resistance of the polyester raw material. The test conditions are: the electron accelerator energy is 10Mev, the temperature is room temperature (25°C), and the environment atmosphere is exposed to ordinary air. The radiation resistance of the sample is as follows:
[0031] When the electron beam radiation dose increases from 0 kGy to 100 kGy, the tensile strength of the pure PBS sample in the non-additive group decreases from about 41 MPa before irradiation to 38 MPa after irradiation; the tensile elongation at break decreases from about 11% before irradiation to about 8% after irradiation; the tensile strength of the composite sample of the present embodiment increases slightly from 33 MPa before irradiation to 35 MPa after irradiation, and the elongation at break increases slightly from about 9% before irradiation to about 10% after irradiation.
[0032] When the electron beam radiation dose increased from 0 kGy to 200 kGy, the tensile strength of the pure PBS sample in the non-additive group decreased significantly from 41 MPa to 20 MPa, and the tensile elongation at break decreased from about 11% to about 2%; the sample of the composite material of this embodiment decreased from 33 MPa to about 27 MPa, and the elongation at break decreased from about 9% to 5%.
[0033] This compounding ratio is achieved within the range of high radiation doses below 200 kGy, effectively alleviating the significant decrease in mechanical strength and toughness of aliphatic polyester PBS caused by increasing radiation doses.
[0034] Example 2
[0035] The preparation process of the radiation-resistant composite material is the same as that of Example 1, and PBS polyester is still used as the main masterbatch, but the ratio is different, PBS is taken as 97%, and the proportion of the additive 3-(2,3-epoxypropoxy)propyltrimethoxysilane is increased to 3%, and other process conditions are the same as those of Example 1.
[0036] When the electron beam radiation dose increases from 0kGy to 100kGy, the tensile strength of the composite sample with this ratio increases from 46Mpa to 47.5Mpa, and the tensile elongation at break decreases from 245% to 25%;
[0037] When the electron beam radiation dose increases from 0kGy to 200kGy, the tensile strength of the composite sample with this ratio remains at around 46Mpa without significant change. The tensile elongation at break decreases from 245% to 20%;
[0038] This compounding ratio significantly maintains the mechanical strength of the polyester composite material sample at a high radiation dose of 100-200kGy almost unchanged, and significantly improves the initial elongation at break of the composite material before irradiation (the elongation at break of the pure PBS sample without addition at 0kGy is about 11%, which is greatly increased to about 245% of the composite material in the added group). The tensile elongation at break of the polyester composite material at a high radiation dose (such as 200kGy in this example) is also significantly maintained (the group without addition is almost completely brittle, with only about 2% tensile elongation at break remaining, and the group with addition always maintains an elongation at break of more than 20%).
[0039] In summary, for the polyester masterbatch PBS, the additives of the present invention can significantly improve the mechanical strength of saturated aliphatic polyesters before radiation, and can significantly alleviate the degradation trend of such polyesters after radiation. The additive feed ratio and processing temperature and other parameters can be adjusted for different saturated aliphatic polyester raw materials according to actual needs.
[0040] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An additive, characterized in that: The additive is suitable for the formulation system of saturated aliphatic polyester to resist ionizing radiation, and contains epoxysiloxane.
2. The additive according to claim 1, characterized in that The saturated aliphatic polyester is a polycarboxylate whose main chain structure is a saturated aliphatic chain structure.
3. The additive according to claim 1, characterized in that The epoxysiloxane is an organic silicon compound having an epoxy group at one end of the molecular chain and an alkoxysilicon structure at the other end, and the intermediate molecular structure connecting the two ends is a saturated CC or CO chain.
4. A saturated aliphatic polyester material resistant to ionizing radiation, characterized in that: The invention comprises the additives as claimed in claims 1 to 3 and a saturated aliphatic polyester.
5. The saturated aliphatic polyester material resistant to ionizing radiation according to claim 4, characterized in that: The epoxysiloxane is added in an amount of 0.1% to 10% relative to the total weight of the feed.
6. The saturated aliphatic polyester material resistant to ionizing radiation according to claim 5, characterized in that: The saturated aliphatic polyester material resistant to ionizing radiation does not contain aromatic hydrocarbon structure and unsaturated olefin unit; the additive formula components can withstand processing temperatures below 300 degrees.
7. A method for preparing a saturated aliphatic polyester material resistant to ionizing radiation according to any one of claims 4 to 6, characterized in that: The steps include: 1) Pre-drying the saturated aliphatic polyester raw material for standby use; 2) adding the epoxysiloxane type additive to the dried saturated aliphatic polyester pure raw material and stirring to mix well; 3) adding the mixed materials into a melting device and mixing them at the mixing temperature of the pure raw material of saturated aliphatic polyester to be processed until they are uniform; 4) The material after the banburying in step 3) is crushed and then re-granulated to obtain a saturated aliphatic polyester modified composite masterbatch.
8. The method for preparing the ionizing radiation resistant saturated aliphatic polyester material according to claim 7, characterized in that: In step 2), the epoxysiloxane is added to the pure raw material of the saturated aliphatic polyester alone, or the epoxysiloxane is added in multiple times during the mixing process of step 3).