Low-light-transmittance medicine bottle and preparation method thereof
High doping is solved by using fluid modifiers of long-chain fatty acids, linear low-density polyethylene and maleic anhydride grafted polyethylene in the bottle masterbatch, and hydroxy hyperbranched polyester on the grafted end of the titanium dioxide surface The problem of rising light transmittance of the medicine bottle caused by titanium dioxide achieves better dispersion and light blocking effects.
Patent Information
- Application Number
- CN202411311855.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-20
AI Technical Summary
High-dose titanium dioxide leads to a decrease in melt flowability and extrusion during the preparation of the masterbatch of the medicine bottle, resulting in an increase in the light transmittance of the medicine bottle, affecting the stability of the medicine.
Add long-chain fatty acids, linear low-density polyethylene and maleic anhydride grafted polyethylene as fluid modifiers to the carrier resin of the masterbatch, and hydroxyl hyperbranched polyester on the graft end of the titanium dioxide surface to improve the dispersion of titanium dioxide. and light blocking effect.
It effectively improves the flowability and extrusion properties of the masterbatch, promotes the uniform dispersion of titanium dioxide, reduces the light transmittance of the medicine bottle, and enhances the light blocking effect.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of pharmaceutical packaging materials, and in particular to a low-transmittance medicine bottle and a preparation method thereof. Background Art
[0002] In the field of pharmaceutical packaging, pharmaceutical packaging bottles are the key barrier to protect drugs from the external environment, and their performance is directly related to the stability and safety of drugs. Among them, light transmittance is one of the important indicators to measure the performance of pharmaceutical packaging bottles. Since many drugs are sensitive to light, especially ultraviolet rays, long-term exposure to light may cause the active ingredients of the drugs to degrade, discolor or produce adverse reactions. Therefore, it is crucial to ensure that pharmaceutical packaging bottles have sufficient light-blocking properties.
[0003] In the current market, in order to improve the light-blocking effect of medicine bottles, a commonly used strategy is to add a large amount of titanium dioxide to the base resin of the medicine bottle. Titanium dioxide, with its excellent light reflection and light absorption capabilities, can significantly reduce the light transmittance of the medicine bottle, thereby effectively protecting the medicine from light damage. However, directly adding titanium dioxide powder to the resin often faces the problem of uneven dispersion, which not only affects the light-blocking effect of the medicine bottle, but may also have an adverse effect on the molding and processing performance of the medicine bottle and the appearance quality of the final product.
[0004] In order to overcome the above defects, the industry usually adopts the method of pre-mixing titanium dioxide with carrier resin to prepare masterbatch. Masterbatch technology helps to improve the dispersibility of titanium dioxide in the base resin and improve its dispersion uniformity through the encapsulation effect of the carrier resin. For example, the patent with publication number CN106905669A discloses a titanium dioxide masterbatch and its preparation method, which records that the amount of titanium dioxide is 30-70%. However, although the high amount of titanium dioxide can enhance the light-blocking effect, the melt fluidity and extrusion of the masterbatch will be significantly reduced. On the one hand, it will cause melt fracture, poor filling in the mold, and appearance defects such as voids, bubbles, and rough surface; on the other hand, poor extrusion will cause uneven dispersion of titanium dioxide, resulting in increased light transmittance of the medicine bottle and affecting the stability of the medicine. This contradictory phenomenon limits the application of high-content titanium dioxide masterbatch in the production of medicine bottles. Summary of the invention
[0005] The present application provides a low-transmittance medicine bottle and a preparation method thereof, which can significantly alleviate the problem of decreased melt fluidity and extrudability caused by high-doped titanium dioxide in the preparation process of masterbatch, resulting in increased transmittance of the medicine bottle.
[0006] In a first aspect, the present application provides a low-transmittance medicine bottle, wherein the raw materials thereof contain 3.5-5wt% masterbatch, and the remainder is high-density polyethylene; in terms of mass percentage, the raw materials of the masterbatch include: Titanium dioxide 40-50%, stabilizer 1-4%, dispersant 2-5%, carrier resin as the balance; The carrier resin includes high-density polyethylene and a fluid modifier in a mass ratio of 100:10-30; the fluid modifier includes long-chain fatty acids, linear low-density polyethylene and maleic anhydride grafted polyethylene in a mass ratio of 5-10:10-20:5-10, and the number of carbon atoms of the long-chain fatty acids is 12-20; at 190°C and 2.16Kg, the melt index of the linear low-density polyethylene is 10-30g / 10min.
[0007] Preferably, the long-chain fatty acid is at least one of palmitic acid, lauric acid or stearic acid.
[0008] Preferably, the grafting rate of the maleic anhydride grafted polyethylene is 1-2%.
[0009] In the present disclosure, the high-density polyethylene used as the raw material of the medicine bottle and the high-density polyethylene used as the carrier resin can be the same high-density polyethylene, or different high-density polyethylenes can be selected.
[0010] Preferably, the high-density polyethylene used as the raw material for medicine bottles has a melt index of 0.1 to 1 g / 10 min at 190°C and 2.16 kg, more preferably 0.2 to 0.5 g / 10 min.
[0011] The medicine bottle raw material disclosed in the present invention can be added with other processing aids of the polyethylene composition according to the actual processing needs, including but not limited to plasticizers, reinforcing agents, lubricants, flame retardants, antistatic agents, nucleating agents, fillers, and pigments. The amounts used are all conventional amounts, or can be adjusted according to the requirements of actual conditions.
[0012] In the preparation and molding of masterbatch extrusion, the following three points need to be paid attention to in order to improve its fluidity. The first is the good flow of the melt in the extruder barrel, and the shearing action of the screw ensures the good dispersion of titanium dioxide; the second is that the melt needs to enter the die head smoothly from the end of the screw to prevent retention and agglomeration, and blockage of the gate; the third is to ensure the compatibility between the components and improve the melting performance of the melt in the screw.
[0013] In order to achieve the above effects, the present application incorporates a fluid modifier into the carrier resin of the masterbatch, which includes long-chain fatty acids, linear low-density polyethylene and maleic anhydride grafted polyethylene. Among them, the linear low-density polyethylene adopts a high melt index material, which can effectively reduce the viscosity of the melt, improve the melt fluidity in the barrel, and help the dispersion of titanium dioxide. Assisted by long-chain fatty acids, the problem of melt retention and blockage at the die entrance can be effectively avoided, and good extrusion can be achieved in the masterbatch preparation process, and the uniformity of titanium dioxide can be improved. Maleic anhydride grafted polyethylene can improve the compatibility between the components of the masterbatch, achieve good dissolution, and have an additional synergistic effect on the improvement of extrusion performance.
[0014] It should be noted that when the carbon number of long-chain fatty acids is less than 12, they are in liquid form and there is a risk of migration and precipitation. Long-chain fatty acids with more than 20 carbon atoms are more difficult to obtain.
[0015] In addition, the melt index of linear low-density polyethylene also needs to be appropriate. When the melt index is low, the fluidity is poor, while if the melt index is too high, the material molecular weight is low and the thermal stability is poor, which is not conducive to improving the extrusion performance.
[0016] Preferably, the surface of the titanium dioxide is grafted with a terminal hydroxyl hyperbranched polyester via an isocyanate silane coupling agent, and the mass ratio of the titanium dioxide, the isocyanate silane coupling agent, and the terminal hydroxyl hyperbranched polyester is 100:1-2:8-15.
[0017] Preferably, the isocyanate silane coupling agent is γ-isocyanate propyl trimethoxy silane and / or γ-isocyanate propyl triethoxy silane.
[0018] Preferably, the hydroxyl value of the hydroxyl-terminated hyperbranched polyester is 200 to 400 mg KOH / g.
[0019] Preferably, the titanium dioxide is rutile titanium dioxide.
[0020] Preferably, the average particle size of the titanium dioxide is 0.1 to 10 microns, more preferably 0.1 to 0.5 microns.
[0021] It should be noted that the content of titanium dioxide in this application should not be higher than 5% to meet the requirements of the national standard on the content of residue on ignition.
[0022] The surface modification disclosed herein has the following effects: First, the grafting of terminal hydroxyl hyperbranched polyester can inhibit the agglomeration tendency of titanium dioxide and ensure the dispersion effect.
[0023] Secondly, while achieving the chemical bonding between titanium dioxide and the terminal hydroxyl hyperbranched polyester, the isocyanate silane coupling agent can consume the nucleation sites on its surface, and cooperate with the terminal hydroxyl hyperbranched polyester with a hyperbranched structure to effectively weaken the effect of titanium dioxide on the crystallization process of polyethylene during the subsequent blow molding of the medicine bottle, which is beneficial to reduce the crystallinity and reduce the transmittance.
[0024] Secondly, the hyperbranched structure of the terminal hydroxyl hyperbranched polyester can form entanglements with the polymer, thereby improving the light-blocking effect and reducing the light transmittance.
[0025] In addition, the terminal hydroxyl hyperbranched polyester is attached to the surface of titanium dioxide, which can play a buffering and protective role, preventing the shearing and extrusion effect of the screw from destroying the light reflection ability of titanium dioxide.
[0026] It should be noted that the hydroxyl value of the terminal hydroxyl hyperbranched polyester needs to be appropriate. Too low hydroxyl value is not conducive to the grafting reaction, and too high hydroxyl value is not conducive to improving compatibility.
[0027] Preferably, an alkyl silane coupling agent is grafted onto the surface of the titanium dioxide, the number of carbon atoms of the alkyl silane coupling agent is 8 to 12, and the mass ratio of the alkyl silane coupling agent to the isocyanate silane coupling agent is 1 to 2:0.5 to 2.
[0028] Preferably, the alkylsilane coupling agent is selected from at least one of octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane and dodecyltriethoxysilane.
[0029] The main purpose of grafting the above alkylsilane coupling agent disclosed in the present invention is to improve the compatibility of the grafted titanium dioxide with the polyethylene substrate. In addition, it can also reduce the friction coefficient of titanium dioxide, which helps to improve the melt fluidity.
[0030] Preferably, the stabilizer comprises calcium stearate and zinc stearate in a mass ratio of 1-2:1-2.
[0031] Preferably, the dispersant is polyethylene wax.
[0032] In a second aspect, the present application provides a method for preparing a low-transmittance medicine bottle, which comprises the following steps: Prepare raw materials according to the raw material ratio described in any one of claims 1 to 9; The masterbatch raw materials are mixed and extruded to obtain masterbatch, and the extruder temperature is set at 200-240°C; The high-density polyethylene and the masterbatch are hot-melted at 200-250°C, injection-molded into a bottle embryo, and the bottle embryo is blow-molded and then taken off the bottle to obtain the bottle.
[0033] In summary, this application has the following beneficial effects: The present application adds a fluid modifier obtained by mixing long-chain fatty acids, linear low-density polyethylene and maleic anhydride grafted polyethylene into the masterbatch carrier resin, which effectively alleviates the problems of poor fluidity and extrusion of the fluid in the barrel and at the point where the barrel enters the die gate during the preparation of the masterbatch at a high titanium dioxide dosage, improves the quality of the masterbatch, promotes the uniform dispersion of titanium dioxide, helps to improve the dispersibility of titanium dioxide in the medicine bottle, exerts its light reflection and light absorption effects, and effectively reduces the light transmittance.
[0034] In addition, the present application can inhibit the agglomeration tendency and nucleation of titanium dioxide, promote the entanglement of titanium dioxide and polymer, prevent shear damage to titanium dioxide, etc., by grafting terminal hydroxyl hyperbranched polyester on the surface of titanium dioxide, thereby effectively improving the light-blocking effect. DETAILED DESCRIPTION Preparation Example
[0035] Preparation Example 1 Modified titanium dioxide, the preparation steps are as follows: In 8L ethanol aqueous solution (ethanol 30wt%) at pH 4, add 16g of γ-isocyanate propyl trimethoxysilane and 10g of n-octyl trimethoxysilane, stir for 10min, then add 1000g of rutile titanium dioxide (D50 particle size is 0.2 micron), stir and react for 20min. Heat to 60℃, add 100g of terminal hydroxyl hyperbranched polyester (hydroxyl value 320mgKOH / g, molecular weight 1000), stir and react for 35min. Separate and filter out titanium dioxide, wash with deionized water until neutral, and obtain modified titanium dioxide.
[0036] Preparation Example 2 Modified titanium dioxide, the preparation steps are as follows: In 8L ethanol aqueous solution (ethanol 30wt%) at pH 4, add 10g of γ-isocyanate propyl trimethoxysilane and 7g of n-octyl trimethoxysilane, stir for 10min, then add 1000g of rutile titanium dioxide (D50 particle size is 0.2 micron), stir and react for 15min. Heat to 55°C, add 80g of terminal hydroxyl hyperbranched polyester (hydroxyl value 220mgKOH / g, molecular weight 6400), stir and react for 35min. Separate and filter out titanium dioxide, wash with deionized water until neutral, and obtain modified titanium dioxide.
[0037] Preparation Example 3 Modified titanium dioxide, the preparation steps are as follows: In 8L ethanol aqueous solution (ethanol 30wt%) at pH 4, add 20g of γ-isocyanate propyl trimethoxysilane and 20g of dodecyl trimethoxysilane, stir for 10min, then add 1000g of rutile titanium dioxide (D50 particle size is 0.3 micron), stir and react for 20min. Heat to 60℃, add 150g of terminal hydroxyl hyperbranched polyester (hydroxyl value 360mgKOH / g, molecular weight 950), stir and react for 40min. Separate and filter out titanium dioxide, wash with deionized water until neutral, and obtain modified titanium dioxide.
[0038] Preparation Example 4 The modified titanium dioxide is different from that of Preparation Example 1 in that n-octyltrimethoxysilane is replaced by an equal amount of γ-isocyanatepropyltrimethoxysilane.
[0039] Preparation Example 5 The modified titanium dioxide is different from that in Preparation Example 1 in that an equal amount of n-octyltrimethoxysilane is used to replace γ-isocyanatepropyltrimethoxysilane.
[0040] Preparation Example 6 The modified titanium dioxide is different from that of Preparation Example 1 in that the terminal hydroxyl hyperbranched polyester is replaced by an equal amount of n-octyltrimethoxysilane. Example
[0041] Example 1, a low light transmittance medicine bottle, the preparation method is as follows: Preparation of masterbatch: Take 10kg of raw materials, the raw material ratio is 48.3% of modified titanium dioxide in Preparation Example 1, 1.5% of calcium stearate, 1.3% of zinc stearate, 3.5% of polyethylene wax, 2.0% of lauric acid, 3.8% of linear low-density polyethylene (melting index is 20g / 10min at 190℃ and 2.16Kg, Vicat softening point is 94℃), 1.5% of maleic anhydride grafted polyethylene (grafting rate is 1.2%), and 38.1% of high-density polyethylene (melting index is 0.35g / 10min at 190℃ and 2.16Kg). Add the raw materials to a high-speed mixer and mix them evenly, then add them to a twin-screw extruder for melt extrusion granulation, and after water cooling, drying, and pelletizing, obtain a masterbatch with an average particle size of 3mm. The extruder temperature was set at 200-240°C, and the temperatures of each section from the feed port to the die were: 200°C, 210°C, 215°C, 220°C, 240°C, 220°C, 215°C, 210°C, 210°C, and 200°C.
[0042] Injection blow molding: 95.5 kg of high-density polyethylene (melt index of 0.35 g / 10 min at 190°C and 2.16 kg) and 4.5 kg of the above masterbatch are hot-melted at 215-235°C, injection-molded into a bottle embryo, and the bottle embryo is blow-molded and then removed from the bottle. The temperature of the extruder section 1 is 215°C, section 2 is 228°C, section 3 is 235°C, section 4 is 235°C, the nozzle is 235°C, and the flow channel is 230°C.
[0043] Example 2, a low light transmittance medicine bottle, the preparation method is as follows: Preparation of masterbatch: Take 10kg of raw materials, the raw material ratio is 40.6% of modified titanium dioxide in Preparation Example 2, 1.7% of calcium stearate, 1.6% of zinc stearate, 2.7% of polyethylene wax, 1.4% of palmitic acid, 3.0% of linear low-density polyethylene (melting index is 25g / 10min at 190℃ and 2.16Kg, Vicat softening point is 91.7℃), 1.5% of maleic anhydride grafted polyethylene (grafting rate is 1.0%), and 47.5% of high-density polyethylene (melting index is 0.35g / 10min at 190℃ and 2.16Kg). Add the raw materials to a high-speed mixer and mix them evenly, then add them to a twin-screw extruder for melt extrusion granulation, and after water cooling, drying, and pelletizing, obtain a masterbatch with an average particle size of 3mm. The extruder temperature was set at 200-240°C, and the temperatures of each section from the feed port to the die were: 200°C, 210°C, 220°C, 230°C, 240°C, 220°C, 215°C, 210°C, 210°C, and 200°C.
[0044] Injection blow molding: 96.5 kg of high-density polyethylene (melt index of 0.35 g / 10 min at 190°C and 2.16 kg) and 3.5 kg of the above masterbatch are hot-melted at 215-235°C, injection-molded into a bottle embryo, and the bottle embryo is blow-molded and then removed from the bottle. The temperature of the extruder section 1 is 215°C, section 2 is 228°C, section 3 is 235°C, section 4 is 235°C, the nozzle is 235°C, and the flow channel is 230°C.
[0045] Example 3, a low light transmittance medicine bottle, the preparation method is as follows: Preparation of masterbatch: Take 10kg of raw materials, the raw material ratio is 48.3% of modified titanium dioxide in Preparation Example 3, 1.5% of calcium stearate, 1.3% of zinc stearate, 3.5% of polyethylene wax, 2.0% of stearic acid, 3.8% of linear low-density polyethylene (melting index is 12g / 10min at 190℃ and 2.16Kg, Vicat softening point is 94℃), 1.5% of maleic anhydride grafted polyethylene (grafting rate is 1.2%), and 38.1% of high-density polyethylene (melting index is 0.23g / 10min at 190℃ and 2.16Kg). Add the raw materials to a high-speed mixer and mix them evenly, then add them to a twin-screw extruder for melt extrusion granulation, and after water cooling, drying, and pelletizing, obtain a masterbatch with an average particle size of 3mm. The extruder temperature was set at 200-240°C, and the temperatures of each section from the feed port to the die were: 200°C, 210°C, 215°C, 220°C, 240°C, 220°C, 215°C, 210°C, 210°C, and 200°C.
[0046] Injection blow molding: 95.0 kg of high-density polyethylene (melt index of 0.35 g / 10 min at 190°C and 2.16 kg) and 5.0 kg of the above masterbatch are hot-melted at 200-235°C, injection-molded into a bottle embryo, and the bottle embryo is blow-molded and then removed from the bottle. The temperature of the extruder section 1 is 200°C, section 2 is 215°C, section 3 is 225°C, section 4 is 235°C, the nozzle is 235°C, and the flow channel is 230°C.
[0047] Example 4, a low transmittance medicine bottle, is different from Example 1 in that the modified titanium dioxide of Preparation Example 1 is replaced by an equal amount of modified titanium dioxide of Preparation Example 4.
[0048] Example 5, a low-transmittance medicine bottle, differs from Example 1 in that the modified titanium dioxide of Preparation Example 1 is replaced by an equal amount of modified titanium dioxide of Preparation Example 5.
[0049] Example 6, a low transmittance medicine bottle, differs from Example 1 in that the modified titanium dioxide of Preparation Example 1 is replaced by an equal amount of modified titanium dioxide of Preparation Example 6. Comparative Example
[0050] Comparative Example 1 is a low-transmittance medicine bottle, which differs from Example 6 in that in the masterbatch raw material, lauric acid is replaced by an equal amount of maleic anhydride grafted polyethylene (grafting rate is 1.2%).
[0051] Comparative Example 2 is a low-transmittance medicine bottle, which differs from Example 6 in that the linear low-density polyethylene is replaced by an equal amount of high-density polyethylene (melt index of 0.35 g / 10 min at 190°C and 2.16 kg) in the masterbatch raw material.
[0052] Comparative Example 3, a low transmittance medicine bottle, is different from Example 6 in that the maleic anhydride grafted polyethylene is replaced by an equal amount of linear low-density polyethylene (melt index of 20 g / 10 min at 190°C and 2.16 kg, Vicat softening point of 94°C) in the masterbatch raw material.
[0053] Comparative Example 4, a low transmittance medicine bottle, is different from Example 6 in that in the masterbatch raw material, lauric acid, linear low density polyethylene and maleic anhydride grafted polyethylene are replaced with an equal amount of high density polyethylene (melt index of 0.35 g / 10 min at 190°C and 2.16 kg). Performance testing
[0054] Test 1: Masterbatch appearance quality Randomly select 50 masterbatches from the masterbatches prepared in each embodiment and comparative example, and observe the surface structure of the extruded product with an optical microscope or an electron microscope to see whether there are appearance defects such as cavities, bubbles, and surface roughness, and calculate the appearance defect rate.
[0055] Test 2: Light transmittance test (1) Sample preparation: Select a sample with uniform thickness, cut a circular section from two or more bottle walls, clean and dry, and do not scratch the surface. If the sample is too small to cover the sample holder, cover the open part with opaque paper or tape. If the length of the sample is longer than the length of the spectrophotometer slit, install the sample on the sample holder and use sticky wax or other simple methods to mount the sample. Be careful to avoid finger marks or other marks on the surface that affect the passage of light.
[0056] (2) Detection method: Place the sample on a light transmission measurement spectrophotometer so that the central axis of the sample is parallel to the slit plane of the spectrophotometer and near the center of the slit. When the sample is placed in the appropriate position, the light beam reaches the sample surface normally and the reflection loss is minimized. With air as a reference, measure the transmittance of the sample in the required spectral region and continuously record it every 40nm in the wavelength range of 290nm-450nm using a recording instrument or a manual instrument.
[0057] Table 1. Test results
[0058] Analysis of test results: It can be seen from the combination of Examples 1 to 6 and Comparative Examples 1 to 4 and Table 1 that the fluid modifier composed of long-chain fatty acids, linear low-density polyethylene and maleic anhydride grafted polyethylene added to the masterbatch in the present application can effectively improve the fluidity and extrudability of the masterbatch raw material melt under high titanium dioxide dosage, while reducing the poor appearance of the masterbatch, promoting the effective dispersion of titanium dioxide, and helping to obtain a HDPE medicine bottle with lower light transmittance. The reason may be that linear low-density polyethylene can reduce the viscosity of the melt in the extruder barrel and improve its fluidity; while long-chain fatty acids can improve the extrudability of the melt when it enters the die from the barrel, preventing the melt from being retained and blocked at the die inlet (screw end); maleic anhydride grafted polyethylene can improve the solubility between the raw materials of the melt and improve the extrudability of the melt.
[0059] Further, in combination with Example 1 and Examples 4 to 6 and Table 1, it can be seen that the present application grafts terminal hydroxyl hyperbranched polyester and alkyl silane coupling agent on the surface of titanium dioxide, which can effectively reduce the light transmittance of the medicine bottle. The reason may be that the terminal hydroxyl hyperbranched polyester has a significant effect on inhibiting the agglomeration tendency and nucleation of titanium dioxide, and can also promote the entanglement of titanium dioxide and polymer, prevent shear damage to titanium dioxide, and improve the light blocking effect.
[0060] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
Claims
1. A low light transmittance medicine bottle, It is characterized in that The raw material contains 3.5-5wt% masterbatch, and the balance is high-density polyethylene; In terms of mass percentage, the raw materials of masterbatch include: Titanium dioxide 40-50%, stabilizer 1-4%, dispersant 2-5%, carrier resin as the balance; The carrier resin includes high-density polyethylene and a fluid modifier in a mass ratio of 100:10-30; the fluid modifier includes long-chain fatty acids, linear low-density polyethylene and maleic anhydride grafted polyethylene in a mass ratio of 5-10:10-20:5-10, and the number of carbon atoms of the long-chain fatty acids is 12-20; at 190°C and 2.16Kg, the melt index of the linear low-density polyethylene is 10-30g / 10min.
2. The medicine bottle according to claim 1, It is characterized in that The long-chain fatty acid is at least one of palmitic acid, lauric acid or stearic acid.
3. The medicine bottle according to claim 1, It is characterized in that The grafting rate of the maleic anhydride grafted polyethylene is 1-2%.
4. The medicine bottle according to claim 1, It is characterized in that The surface of the titanium dioxide is grafted with terminal hydroxyl hyperbranched polyester through an isocyanate silane coupling agent, and the mass ratio of the titanium dioxide, the isocyanate silane coupling agent and the terminal hydroxyl hyperbranched polyester is 100:1-2:8-15.
5. The medicine bottle according to claim 4, It is characterized in that The isocyanate silane coupling agent is γ-isocyanate propyl trimethoxy silane and / or γ-isocyanate propyl triethoxy silane.
6. The medicine bottle according to claim 4, It is characterized in that The hydroxyl value of the terminal hydroxyl hyperbranched polyester is 200 to 400 mgKOH / g.
7. The medicine bottle according to claim 4, It is characterized in that The titanium dioxide surface is also grafted with an alkyl silane coupling agent, the carbon number of the alkyl silane coupling agent is 8-12, and the mass ratio of the alkyl silane coupling agent to the isocyanate silane coupling agent is 1-2:0.5-2.
8. The medicine bottle according to claim 1, It is characterized in that The stabilizer comprises calcium stearate and zinc stearate in a mass ratio of 1-2:1-2.
9. The medicine bottle according to claim 1, It is characterized in that The dispersant is polyethylene wax.
10. A method for preparing a low-transmittance medicine bottle, It is characterized in that The steps include: Prepare raw materials according to the raw material ratio described in any one of claims 1 to 9; The masterbatch raw materials are mixed and extruded to obtain masterbatch, and the extruder temperature is set at 200-240°C; The high-density polyethylene and the masterbatch are hot-melted at 200-250°C, injection-molded into a bottle embryo, and the bottle embryo is blow-molded and then taken off the bottle to obtain the bottle.
Citation Information
Patent Citations
Colored plastic ampoule bottle and preparation method thereof
CN115558189A
Preparation method of modified titanium dioxide for polyethylene shading master batch
CN117024991A
Polyethylene resin composition and medical container comprising the same
JP2015074744A
Titanuim Dioxide Pigments, Process For The Production Thereof,And Resin Compostions Containing The Pigments
US20070295244A1