Antibacterial PVC composition and preparation method thereof
By using a combination of fatty alkyl dihydroxyethyl quaternary ammonium salt and impact modifier, the problem of the reduction of antibacterial ability of small molecule antibacterial agents in high temperature and sunlight is solved, and the long-term antibacterial effect in PVC materials is achieved.
Patent Information
- Application Number
- CN202411392796.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-10-08
AI Technical Summary
Small-molecule antibacterial agents are prone to evaporation or decomposition under sunlight radiation or high temperature environments, resulting in a decrease in antibacterial ability and cannot meet the long-term antibacterial needs.
Fatty alkyl dihydroxyethyl quaternary ammonium salt is used as an antibacterial agent, and hydrogen bond cross-linking is formed with the impact modifier in PVC resin to improve the heat resistance and stability of the antibacterial agent, while introducing imidazole salt and hydroxyl group. Monomers to enhance antibacterial effects.
It effectively improves the heat resistance and long-term antibacterial properties of antibacterial agents, ensuring good antibacterial effect under high temperature and sunlight irradiation conditions.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of PVC materials, and in particular to an antibacterial PVC composition and a preparation method thereof. Background Art
[0002] Antibacterial PVC materials play an outstanding role in the fields of medical products, food processing equipment, packaging materials, public facilities, chemical equipment, etc. Antibacterial PVC materials are materials prepared by adding antibacterial agents and other additives to PVC resins using a blending process. Antibacterial agents are usually small molecule compounds that can gradually migrate and precipitate to the surface of PVC products to form an antibacterial film due to their low compatibility with the base resin, thereby exerting a good antibacterial effect. Such small molecule antibacterial agents include but are not limited to quaternary ammonium antibacterial agents (such as benzalkonium chloride), silver ion antibacterial agents, and phenolic antibacterial agents (such as triclosan).
[0003] However, small molecule antimicrobial agents are prone to volatilization or decomposition under outdoor sunlight or high temperature application environments such as chemical plants and food factories, which can reduce their antimicrobial ability or even make them ineffective. This not only shortens the service life of antimicrobial PVC products, but also fails to meet the long-term antimicrobial needs in various scenarios. Summary of the invention
[0004] In order to solve the problem that the antibacterial ability of PVC products using small molecule antibacterial agents decreases under sunlight radiation or high temperature environment, the present application provides an antibacterial PVC composition and a preparation method thereof.
[0005] In a first aspect, the present application provides an antibacterial PVC composition, which comprises the following components in parts by weight: 100 parts of PVC resin, 1-3 parts of fatty alkyl dihydroxyethyl quaternary ammonium salt, 25-35 parts of filler, 5-10 parts of impact modifier, 1-3 parts of lubricant, and 10-20 parts of plasticizer; the raw materials of the fatty alkyl dihydroxyethyl quaternary ammonium salt include fatty amine, ethylene oxide and quaternary ammonium modifier in a molar ratio of 1:2-2.5:1-1.5; the carbon number of the fatty amine is 6-18.
[0006] Preferably, the preparation method of the fatty alkyl dihydroxyethyl quaternary ammonium salt comprises the following steps: Fatty amines are mixed with ethylene oxide for addition reaction to obtain bis(2-hydroxyethyl) fatty amines; The bis(2-hydroxyethyl) fatty amine and the quaternary ammonium modifier are subjected to a quaternization reaction to prepare a fatty alkyl dihydroxyethyl quaternary ammonium salt.
[0007] Preferably, the fatty amine has 8 to 12 carbon atoms.
[0008] Preferably, the quaternary ammonium modifier is benzyl chloride.
[0009] Preferably, the temperature of the addition reaction is 140-160° C., and the reaction time is 3-5 h.
[0010] The antibacterial agent of the present application is a fatty alkyl dihydroxyethyl quaternary ammonium salt, which belongs to a cationic quaternary ammonium salt antibacterial agent, and can interact with lipids on the cell membrane to destroy the integrity of the cell membrane, causing leakage of cell contents, thereby achieving an antibacterial and bactericidal effect. In particular, the fatty alkyl dihydroxyethyl quaternary ammonium salt of the present application has two hydroxyl groups. After migrating to the PVC surface, the hydroxyl groups can be cross-linked to a certain extent through hydrogen bonding, thereby improving the heat resistance of the antibacterial agent, and helping the antibacterial agent to maintain a good antibacterial effect under sunlight irradiation or high temperature environment.
[0011] It should be noted that the use of fatty amines with longer carbon chains is beneficial to improving the heat resistance of the obtained fatty alkyl dihydroxyethyl quaternary ammonium salts, but its antibacterial effect decreases. The reason may be that with the increase in carbon chain length, the adsorption capacity and lipophilicity of bacteria will increase; but it also causes the hydrophilic-hydrophobic balance of the antibacterial agent to change, causing a decrease in bactericidal and antibacterial ability. In addition, it also leads to an increase in the volume of the antibacterial agent, resulting in changes in its ability to penetrate the bacterial cell wall or cytoplasmic membrane.
[0012] Preferably, the impact modifier is prepared by free radical copolymerization, and the raw materials for the copolymerization reaction include alkyl acrylate, styrene and imidazole salt having unsaturated olefin groups in a mass ratio of 40 to 60:20 to 40:5 to 10.
[0013] Preferably, the acrylic alkyl ester monomer is selected from one or more of ethyl acrylate, propyl acrylate, butyl acrylate, isooctyl acrylate and heptyl acrylate.
[0014] Preferably, the imidazole salt having an unsaturated olefin group is an allyl imidazole salt and / or a vinyl imidazole salt.
[0015] Exemplarily, the allyl imidazole salt is selected from one or more of 1-allyl-3-methylimidazolium chloride, 1-allyl-3-butylimidazolium chloride, and 1-allyl-3-butylimidazolium tetrafluoroborate.
[0016] Exemplarily, the vinyl imidazole salt is selected from one or more of 1-vinyl-3-methyl imidazole chloride, 1-vinyl-3-methyl imidazole nitrate, 1-vinyl-3-propyl imidazole nitrate, 1-vinyl-3-propyl imidazole methanesulfonate, and 1-vinyl-3-butyl imidazole chloride.
[0017] Preferably, the raw materials for the copolymerization reaction further include hydroxy acrylate, and the mass ratio of the alkyl acrylate to the hydroxy acrylate is 40-60:5-15.
[0018] Preferably, the hydroxyacrylate is selected from at least one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate and hydroxybutyl methacrylate.
[0019] The main function of the impact modifier is to improve the problem of increased brittleness and insufficient flexibility of the material after the addition of additives. The introduction of imidazole salts into the impact modifier can give it good antibacterial ability, and because the impact modifier has good compatibility with PVC resin, it is easy to form a dispersed phase in the PVC resin and is not easy to migrate and precipitate, thereby exerting a certain degree of long-term antibacterial effect. In addition, the application of hydroxy acrylate can introduce hydroxyl groups into the PVC resin, restrain the migration of small molecule antibacterial agents through hydrogen bonding, control their outward precipitation rate, reduce the loss of small molecule antibacterial agents, and improve their long-term antibacterial effect.
[0020] Preferably, the preparation method of the impact modifier is as follows: Add emulsifier, alkyl acrylate, hydroxy acrylate, imidazole salt with unsaturated olefin group and neutralizer into deionized water, stir and dissolve to obtain aqueous phase material for later use; Mix styrene and molecular weight regulator evenly to obtain oil phase material for later use; Under the condition of vacuum degree lower than -0.09MPa, add water phase material and 5-10wt% of oil phase material, heat up to 45-55°C, add 20-30wt% of redox initiator, continue to heat up, control the reaction temperature to 60-65°C, react for 10-30min, then drop the remaining oil phase material and redox initiator; keep warm at 65-70°C for 1-2h after the addition is completed, adjust the pH to 5-6 with ammonia water after the insulation, and degassing; then cool to below 45°C, adjust the pH to 6.5-7.5 with ammonia water, filter the material, condense, wash and dry to obtain the product.
[0021] Exemplarily, the oxidant is one or more of dibenzoyl peroxide, potassium persulfate or ammonium persulfate.
[0022] Exemplarily, the reducing agent is selected from one or more of ferrous sulfate, ascorbic acid, triethylenetetramine, and tetraethylenepentamine.
[0023] Preferably, the emulsifier is selected from nonionic emulsifiers.
[0024] Exemplarily, the nonionic emulsifier is fatty alcohol polyoxyethylene ether or fatty acid polyoxyethylene ester.
[0025] Exemplarily, the neutralizing agent is aqueous ammonia.
[0026] Exemplarily, the molecular weight regulator is selected from one or more of tert-dodecyl mercaptan, isooctyl 3-mercaptopropionate, and ethyl 3-mercaptobutyrate.
[0027] Preferably, the redox initiator comprises an oxidizing agent and a reducing agent in a molar ratio of 1:1.
[0028] The fillers, plasticizers and lubricants in the present application are conventionally selected in the art and are not particularly limited.
[0029] Exemplarily, the filler is one or more of calcium carbonate, barium sulfate, carbon black, talc, titanium dioxide, and PMMA.
[0030] Exemplarily, the plasticizer is one or more of an ester plasticizer, an aliphatic plasticizer, an epoxy ester plasticizer, and a phosphate ester plasticizer.
[0031] Exemplarily, the plasticizer is an ester plasticizer, including but not limited to one or more of dioctyl phthalate (DOP), diisooctyl phthalate, dioctyl adipate (DOA), and dioctyl sebacate.
[0032] Exemplarily, the lubricant is one or more of monoglyceride, polyethylene wax, oxidized polyethylene wax, montan wax, polyester wax, and paraffin wax.
[0033] In a second aspect, the present application provides a method for preparing an antibacterial PVC composition, which comprises the following steps: According to the raw material ratio of any of the above-mentioned PVC compositions, PVC resin, filler, fatty alkyl dihydroxyethyl quaternary ammonium salt, impact modifier, lubricant and plasticizer are weighed and added into a blender, and stirred evenly at a temperature of 110-130° C.; The uniformly stirred raw materials are passed through a twin-screw extruder to be melt-extruded and granulated at 140-160° C. to prepare an antibacterial PVC composition.
[0034] In summary, this application has the following beneficial effects: The present application obtains a small molecule antibacterial agent with good heat resistance by preparing a small molecule quaternary ammonium salt antibacterial agent with dihydroxyl groups, which effectively alleviates the problem that the antibacterial performance of small molecule antibacterial agents on the surface of PVC products is easily reduced due to high temperature and ultraviolet radiation. Furthermore, by introducing imidazole salts and hydroxyl monomers into the impact modifier, on the one hand, the imidazole salts can play a long-term antibacterial role; on the other hand, the migration rate of the small molecule antibacterial agent can be reduced by hydrogen bonding with the hydroxyl group of the small molecule antibacterial agent, thereby improving the long-term antibacterial effect. DETAILED DESCRIPTION Preparation examples of raw materials and / or intermediates
[0035] Preparation Example 1-1 Fatty alkyl dihydroxyethyl quaternary ammonium salt, the preparation method is as follows: 185.3 g of dodecylamine (1 mol) was added into a reaction kettle equipped with a pressure gauge and a thermometer, and 106.8 mL of ethylene oxide (density 0.907 g / L) was introduced. The mixture was stirred and heated to 160°C for addition reaction. The reaction lasted for 2 hours. After the temperature and pressure were stabilized, the mixture was cooled and discharged to obtain bis(2-hydroxyethyl)lauramine.
[0036] Add ethanol to the reaction kettle, then add the bis(2-hydroxyethyl)lauramine prepared above, stir and heat to 70°C, add 164.6g of benzyl chloride dropwise to the reaction kettle, the addition should be completed within 10 minutes, reflux for 28 hours, evaporate the ethanol under reduced pressure to obtain fatty alkyl dihydroxyethyl quaternary ammonium salt.
[0037] Preparation Example 1-2 Fatty alkyl dihydroxyethyl quaternary ammonium salt, the preparation method is as follows: 185.3 g of dodecylamine (1 mol) was added into a reaction kettle equipped with a pressure gauge and a thermometer, and 97.1 mL of ethylene oxide (density 0.907 g / L) was introduced. The mixture was stirred and heated to 140°C for an addition reaction. The reaction lasted for 3 hours. After the temperature and pressure were stabilized, the mixture was cooled and discharged to obtain bis(2-hydroxyethyl)lauramine.
[0038] Add ethanol to the reaction kettle, then add 130g of bis(2-hydroxyethyl)lauramine, stir and heat to 75°C, add benzyl chloride dropwise to the reaction kettle, reflux for 24h, and evaporate the ethanol under reduced pressure to obtain fatty alkyl dihydroxyethyl quaternary ammonium salt.
[0039] Preparation Example 1-3 Fatty alkyl dihydroxyethyl quaternary ammonium salt, the preparation method is as follows: 129.2 g of octylamine (1 mol) was added into a reaction kettle equipped with a pressure gauge and a thermometer, and 121.4 mL of ethylene oxide (density 0.907 g / L) was introduced. The mixture was stirred and heated to 140°C for an addition reaction. The reaction lasted for 3 hours. After the temperature and pressure were stabilized, the mixture was cooled and discharged to obtain bis(2-hydroxyethyl)octylamine.
[0040] Add ethanol to the reaction kettle, then add the bis(2-hydroxyethyl)octylamine prepared above, stir and heat to 65°C, add 189.9g of benzyl chloride dropwise to the reaction kettle, the addition should be completed within 20 minutes, reflux for 30 hours, evaporate the ethanol under reduced pressure to obtain fatty alkyl dihydroxyethyl quaternary ammonium salt.
[0041] Preparation Example 1-4 Fatty alkyl dihydroxyethyl quaternary ammonium salt, the preparation method is as follows: 241.5 g of hexadecylamine (1 mol) was added into a reaction kettle equipped with a pressure gauge and a thermometer, and 106.8 mL of ethylene oxide (density 0.907 g / L) was introduced. The mixture was stirred and heated to 160°C for addition reaction. The reaction lasted for 2 hours. After the temperature and pressure were stabilized, the mixture was cooled and discharged to obtain bis(2-hydroxyethyl)palmitamine.
[0042] Add ethanol to the reaction kettle, then add the bis(2-hydroxyethyl)palmitamine prepared above, stir and heat to 70°C, add 164.6g of benzyl chloride dropwise to the reaction kettle, the addition should be completed within 10 minutes, reflux for 28 hours, evaporate the ethanol under reduced pressure to obtain fatty alkyl dihydroxyethyl quaternary ammonium salt.
[0043] Preparation Example 1-5 Fatty alkyl dihydroxyethyl quaternary ammonium salt, the preparation method is as follows: 269.5 g of octadecylamine (1 mol) was added into a reaction kettle equipped with a pressure gauge and a thermometer, and 106.8 mL of ethylene oxide (density 0.907 g / L) was introduced. The mixture was stirred and heated to 160°C for addition reaction. The reaction lasted for 2 hours. After the temperature and pressure were stabilized, the mixture was cooled and discharged to obtain bis(2-hydroxyethyl)stearylamine.
[0044] Add ethanol to the reaction kettle, then add the bis(2-hydroxyethyl)stearylamine prepared above, stir and heat to 70°C, add 164.6g of benzyl chloride dropwise to the reaction kettle, the addition should be completed within 10 minutes, reflux for 28 hours, evaporate the ethanol under reduced pressure to obtain fatty alkyl dihydroxyethyl quaternary ammonium salt.
[0045] Preparation Example 2-1 Impact modifier, the preparation method is as follows: Dissolve fatty alcohol polyoxyethylene ether in deionized water to prepare a 3wt% emulsifier solution, add 490g butyl acrylate, 125g hydroxyethyl acrylate, 80g 1-allyl-3-methylimidazole chloride, and 0.6g 25wt% ammonia water, stir and dissolve, and prepare an aqueous phase material for use.
[0046] 280 g of styrene and 1 g of a molecular weight regulator (ethyl 3-mercaptobutyrate) were mixed evenly to prepare an oil phase material for later use.
[0047] Under the condition of vacuum degree lower than -0.09MPa, add the above-mentioned water phase material and 10wt% oil phase material into the reactor, heat to 50℃, add 30wt% redox initiator, continue to heat, control the reaction temperature to 60℃, react for 20min, then drop the remaining oil phase material and redox initiator; keep warm at 70℃ for 1h after the addition, adjust pH to 6 with ammonia water after the heat preservation, degassing; then cool to below 45℃, adjust pH to 7 with ammonia water, filter the material, condense, wash and dry to obtain. Among them, the oxidant of the redox initiator is benzoyl peroxide, and the reducing agent is triethylenetetramine, and the molar ratio is 1:1.
[0048] Preparation Example 2-2 Impact modifier, the preparation method is as follows: Dissolve fatty alcohol polyoxyethylene ether in deionized water to prepare a 3wt% emulsifier solution, add 400g butyl acrylate, 150g hydroxyethyl methacrylate, 55g 1-allyl-3-methylimidazole chloride, and 0.6g 25wt% ammonia water, stir and dissolve to prepare an aqueous phase material for use.
[0049] 370 g of styrene and 1.2 g of molecular weight regulator (ethyl 3-mercaptobutyrate) were mixed evenly to prepare an oil phase material for use.
[0050] Under the condition of vacuum degree lower than -0.09MPa, add the above-mentioned water phase material and 5wt% oil phase material into the reactor, heat to 50℃, add 20wt% redox initiator, continue to heat, control the reaction temperature to 65℃, react for 20min, drop the remaining oil phase material and redox initiator; keep warm at 70℃ for 1h after the addition, adjust pH to 6 with ammonia water after the heat preservation, degassing; cool to below 45℃, adjust pH to 7 with ammonia water, filter the material, condense, wash and dry to obtain. The oxidant of the redox initiator is benzoyl peroxide, and the reducing agent is ferrous sulfate, with a molar ratio of 1:1.
[0051] Preparation Example 2-3 Impact modifier, the preparation method is as follows: Dissolve fatty alcohol polyoxyethylene ether in deionized water to prepare a 3wt% emulsifier solution, add 580g butyl acrylate, 100g hydroxyethyl acrylate, 100g 1-vinyl-3-methylimidazole nitrate, and 0.6g 25wt% ammonia water, stir and dissolve to prepare an aqueous phase material for use.
[0052] 220 g of styrene and 1 g of a molecular weight regulator (ethyl 3-mercaptobutyrate) were mixed evenly to prepare an oil phase material for later use.
[0053] Under the condition of vacuum degree lower than -0.09MPa, add the above-mentioned water phase material and 10wt% oil phase material into the reactor, heat to 55℃, add 30wt% redox initiator, continue to heat, control the reaction temperature to 60℃, react for 30min, then drop the remaining oil phase material and redox initiator; keep warm at 65℃ for 2h after the addition, adjust pH to 6 with ammonia water after the heat preservation, degassing; cool to below 45℃, adjust pH to 7 with ammonia water, filter the material, condense, wash and dry to obtain. The oxidant of the redox initiator is benzoyl peroxide, and the reducing agent is triethylenetetramine, and the molar ratio is 1:1.
[0054] Preparation Example 2-4 The impact modifier is different from that of Preparation Example 2-1 in that 1-allyl-3-methylimidazole chloride is replaced by an equal amount of butyl acrylate.
[0055] Preparation Example 2-5 The impact modifier is different from that of Preparation Example 2-1 in that hydroxyethyl acrylate is replaced by an equal amount of butyl acrylate. Example
[0056] Example 1, an antibacterial PVC composition, the preparation steps are as follows: Take 1000g SG-5 type PVC resin, 20g fatty alkyl dihydroxyethyl quaternary ammonium salt of Preparation Example 1-1, 280g calcium carbonate (D50 particle size is 10 microns), 130g impact modifier of Preparation Example 2-1, 20g polyethylene wax, 130g dioctyl phthalate, mix, add to a high-speed blender, and stir evenly at 120°C.
[0057] The uniformly stirred raw materials are added to a twin-screw extruder, and melt-extruded and granulated at 140-160° C. to obtain an antibacterial resistant PVC composition. The temperature of the first zone of the screw extruder is 140-150° C., the temperature of the second zone is 145-155° C., the temperature of the third zone is 155-160° C., the temperature of the fourth zone is 150-160° C., and the temperature of the fifth zone is 140-150° C.
[0058] Example 2, an antibacterial PVC composition, the preparation steps are as follows: Take 1000g SG-7 type PVC resin, 30g fatty alkyl dihydroxyethyl quaternary ammonium salt of Preparation Example 1-2, 250g calcium carbonate (D50 particle size is 10 microns), 130g impact modifier of Preparation Example 2-2, 12g polyethylene wax, 100g dioctyl phthalate, mix, add to a high-speed blender, and stir evenly at 120°C.
[0059] The uniformly stirred raw materials are added to a twin-screw extruder, and melt-extruded and granulated at 140-160° C. to obtain an antibacterial resistant PVC composition. The temperature of the first zone of the screw extruder is 140-150° C., the temperature of the second zone is 145-155° C., the temperature of the third zone is 150-160° C., the temperature of the fourth zone is 155-160° C., and the temperature of the fifth zone is 140-155° C.
[0060] Example 3, an antibacterial PVC composition, the preparation steps are as follows: Take 1000g SG-5 type PVC resin, 10g fatty alkyl dihydroxyethyl quaternary ammonium salt of Preparation Example 1-3, 350g calcium carbonate (D50 particle size is 10 microns), 130g impact modifier of Preparation Example 2-3, 30g polyethylene wax, 180g dioctyl phthalate, mix, add to a high-speed blender, and stir evenly at 130°C.
[0061] The uniformly stirred raw materials are added to a twin-screw extruder, and melt-extruded and granulated at 140-160° C. to obtain an antibacterial resistant PVC composition. The temperature of the first zone of the screw extruder is 140-150° C., the temperature of the second zone is 145-155° C., the temperature of the third zone is 150-160° C., the temperature of the fourth zone is 155-160° C., and the temperature of the fifth zone is 150-155° C.
[0062] Example 4, an antibacterial PVC composition, is different from Example 1 in that an equal amount of the fatty alkyl dihydroxyethyl quaternary ammonium salt of Preparation Example 1-4 is used to replace the fatty alkyl dihydroxyethyl quaternary ammonium salt of Preparation Example 1-1.
[0063] Example 5, an antibacterial PVC composition, is different from Example 1 in that an equal amount of the fatty alkyl dihydroxyethyl quaternary ammonium salt of Preparation Example 1-5 is used to replace the fatty alkyl dihydroxyethyl quaternary ammonium salt of Preparation Example 1-1.
[0064] Example 6, an antibacterial PVC composition, is different from Example 1 in that an equal amount of the impact modifier of Preparation Example 2-4 is used to replace the impact modifier of Preparation Example 2-1.
[0065] Example 7, an antibacterial PVC composition, differs from Example 1 in that an equal amount of the impact modifier of Preparation Example 2-5 is used to replace the impact modifier of Preparation Example 2-1. Comparative Example
[0066] Comparative Example 1 is an antibacterial PVC composition, which is different from Example 4 in that an equal amount of dodecyltrimethylammonium chloride is used to replace the fatty alkyl dihydroxyethyl quaternary ammonium salt of Preparation Example 1-1.
[0067] Comparative Example 2 is an antibacterial PVC composition, which is different from Example 4 in that an equal amount of benzalkonium chloride is used to replace the fatty alkyl dihydroxyethyl quaternary ammonium salt of Preparation Example 1-1. Performance testing
[0068] PVC antibacterial performance test (1) According to the provisions of the film method in GB / T 31402-2015 "Test Method for Antibacterial Performance of Plastic Surfaces", the antibacterial rate of the sample was tested for 24 hours, and the test bacteria were Staphylococcus aureus (ATCC 6538P) and Escherichia coli (ATCC8739). The sample was injection molded and cut from the PVC composition of the above embodiment and comparative example. The sample size was 50mm×50mm. Five samples were prepared for each group of samples. Before inoculating the bacterial solution, the samples were placed in a constant temperature and humidity environment of 25±2℃ and 50±5%RH for 7 days. The total number of colonies was determined by referring to the counting method of GB / T4789.2-2003. The calculation formula for the antibacterial rate is as follows: R (%) = (BC) / B × 100% Where: R-antibacterial rate, %; B-average number of recovered bacteria in blank control samples, cfu / piece; C- Average number of recovered bacteria in antibacterial plastic samples, cfu / piece.
[0069] (2) Prepare the sample according to the method in test (1). Before inoculating the bacterial solution, place the sample in a constant temperature and humidity environment of 60±2℃ and 50±5%RH for 7 days, and then irradiate it under a QUV xenon lamp (light source is D65-10) for 48 hours. Measure the antibacterial rate after photothermal treatment to characterize the tolerance of the antibacterial agent to sunlight radiation and high temperature.
[0070] (3) Prepare the sample according to the method in (1), and place it in a constant temperature and humidity environment at 25±2℃ and 50±5%RH for 7 days. Then add it to 500mL sterile saline, sterilize it at 120℃, and add 5x10 5 cfu / mL of bacterial solution (the strain is Escherichia coli ATCC 8739), and after placing it at 30°C for 180 days, the antibacterial rate of the sample was tested again to characterize its long-term antibacterial performance.
[0071] Table 1. Antibacterial performance test results
[0072] Analysis of test results: Combining Examples 1 to 7 and Comparative Examples 1 to 2 and Table 1, it can be seen that the small molecule quaternary ammonium salt antibacterial agent of the present application has high stability under light and high temperature environment. After it is precipitated onto the surface of the PVC surface material, it can maintain a more excellent bactericidal and antibacterial effect after photothermal treatment.
[0073] It can be seen from Examples 1 to 3 and Comparative Examples 4 to 5 and Table 1 that the fatty alkyl dihydroxyethyl quaternary ammonium salt of the present application uses fatty amines with shorter alkyl chains as raw materials, especially fatty amines with no more than 12 carbon atoms, which helps to improve its short-term and long-term antibacterial ability.
[0074] It can be seen from Examples 1 to 3 and Comparative Examples 6 to 7 and Table 1 that the introduction of imidazole salts and hydroxyl groups into the impact modifier can help improve its long-term antibacterial ability.
[0075] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An antibacterial PVC composition, characterized in that: The composition comprises the following components in parts by weight: 100 parts of PVC resin, 1-3 parts of fatty alkyl dihydroxyethyl quaternary ammonium salt, 25-35 parts of filler, 5-10 parts of impact modifier, 1-3 parts of lubricant, and 10-20 parts of plasticizer; the raw materials of the fatty alkyl dihydroxyethyl quaternary ammonium salt include fatty amine, ethylene oxide and quaternary ammonium modifier in a molar ratio of 1:2-2.5:1-1.5; the carbon number of the fatty amine is 6-18.
2. The composition according to claim 1, characterized in that The preparation method of the fatty alkyl dihydroxyethyl quaternary ammonium salt comprises the following steps: Fatty amines are mixed with ethylene oxide for addition reaction to obtain bis(2-hydroxyethyl) fatty amines; The bis(2-hydroxyethyl) fatty amine and the quaternary ammonium modifier are subjected to a quaternization reaction to prepare a fatty alkyl dihydroxyethyl quaternary ammonium salt.
3. The composition according to claim 1, characterized in that The carbon number of the fatty amine is 8-12.
4. The composition according to claim 1, characterized in that The quaternary ammonium modifier is benzyl chloride.
5. The composition according to claim 2, characterized in that The temperature of the addition reaction is 140-160° C., and the reaction time is 3-5 hours.
6. The composition according to claim 1, characterized in that The impact modifier is prepared by free radical copolymerization, and the raw materials for the copolymerization reaction include alkyl acrylate, styrene and imidazole salt with unsaturated olefin groups in a mass ratio of 40-60:20-40:5-10.
7. The composition according to claim 6, characterized in that The acrylic alkyl ester monomer is selected from one or more of ethyl acrylate, propyl acrylate, butyl acrylate, isooctyl acrylate and heptyl acrylate.
8. The composition according to claim 6, characterized in that The imidazole salt having an unsaturated olefin group is an allyl imidazole salt and / or a vinyl imidazole salt.
9. The composition according to claim 6, characterized in that The raw materials for the copolymerization reaction also include hydroxy acrylate, and the mass ratio of the alkyl acrylate to the hydroxy acrylate is 40-60:5-15.
10. A method for preparing an antibacterial PVC composition, characterized in that: The steps include: According to the raw material ratio described in any one of claims 1 to 9, weigh PVC resin, filler, fatty alkyl dihydroxyethyl quaternary ammonium salt, impact modifier, lubricant and plasticizer, add them into a blender, and stir them evenly at a temperature of 110 to 130° C.; The uniformly stirred raw materials are passed through a twin-screw extruder to be melt-extruded and granulated at 140-160° C. to prepare an antibacterial PVC composition.
Citation Information
Patent Citations
Method for preparing antibacterial finishing agent
CN108252096A
Preparation method of quaternary ammonium salt
CN115304501A
Antibacterial plastic and preparation process thereof
CN115386181A
High-temperature-resistant low-temperature-resistant antibacterial PVC (polyvinyl chloride) material and preparation method thereof
CN117551324A
Thermoplastic polymer composition excellent in antistatic and antibacterial properties
JP1997111129A