TPU (thermoplastic polyurethane) hot melt powder modified waterborne polyurethane resin and preparation method thereof

Through the preparation of TPU hot melt powder modified water-based polyurethane resin, the problem of insufficient bonding and washing resistance of existing water-based polyurethane resins is solved, and higher bonding and washing resistance are achieved, meeting industrial needs, and Maintain adhesion in humid environments.

CN118994879AInactive Publication Date: 2024-11-22NANTONG NAR MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311748006.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-19
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing water-based polyurethane resins have insufficient adhesive strength and water washing resistance, which cannot meet industrial needs, and the comprehensive performance of their coating films is poor.

Method used

Using TPU hot melt powder to modify the aqueous polyurethane resin, the mixture of raw material combination and process steps in specific proportions, including deionized water, isocyanate, oligomer polyol, chain extender, TPU hot melt powder, salt forming agent and catalyst With reaction, a modified aqueous polyurethane resin with high viscosity and water-resistant properties was prepared.

Benefits of technology

It improves the product's adhesion and washing resistance, meets industrial needs, and maintains adhesion in dark and humid environments, reduces adhesive marks, and improves the comprehensive performance of the paint.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses TPU (thermoplastic polyurethane) hot melting powder modified waterborne polyurethane resin and a preparation method thereof. The TPU hot melting powder modified waterborne polyurethane resin is prepared from the following raw materials in parts by weight: 30 to 55 parts of deionized water, 8 to 30 parts of diisocyanate, 22 to 45 parts of oligomer polyol, 0.1 to 3.2 parts of chain extender, 0.1 to 3.2 parts of hydrophilic chain extender, 3 to 35 parts of TPU hot melting powder, 0.2 to 0.6 part of salt-forming agent and 0.06 to 0.5 part of catalyst. The grain size of the TPU hot melting powder is less than or equal to 85 microns, the melting point range is 93-107 DEG C, and the heat bonding temperature is 145-165 DEG C. According to the TPU hot-melt powder modified waterborne polyurethane resin and the preparation method thereof, the modified waterborne polyurethane resin is prepared by adding medium-high temperature TPU hot-melt powder, so that the binding power of a product is increased, and the washing resistance is also improved, so that the comprehensive performance of the product is improved; due to the fact that the humidity of the adhesive is large, the adhesive can play a better role in a dark and humid environment, the adhesiveness is more durable, the gloss is not strong, and the adhesive looks like after being used and does not have too large adhesion traces.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermoplastic polyurethane, in particular to a TPU hot-melt powder modified waterborne polyurethane resin and a preparation method thereof. Background Art

[0002] The thermal transfer process is to melt the various patterns on the transfer film and transfer them to the substrate by heating. The thermal transfer film includes a carrier layer, a release layer, a protective layer, an ink layer, and an adhesive layer. The coatings are closely connected and affect each other. Among them, the adhesive layer must have high adhesion, water washing resistance, boiling resistance and chemical resistance. In the production process of hot melt powder modified waterborne polyurethane resin, deionized water, diisocyanate, oligomer polyols and various catalysts need to be put into the reactor for stirring and mixing. At the same time, the outer jacket heat exchanger is used for heating or cooling to promote the production efficiency of the modified waterborne polyurethane resin and ensure product quality.

[0003] Waterborne polyurethane resin has the advantages of high hardness, strong adhesion, corrosion resistance, good solvent resistance, and low VOC content, which meets the "three prerequisites" and "four E principles" for the development of the coating industry. However, general polyurethane emulsions have poor self-thickening properties, low solid content, poor water resistance of latex films, low gloss, and poor overall performance of coatings. In order to better improve the overall performance of waterborne polyurethane coatings and expand the scope of application, WPU emulsions need to be appropriately modified. At present, its modification methods can be roughly divided into four categories: improving monomers and synthesis processes, adding additives, implementing cross-linking, and optimizing compounding.

[0004] The water-based resin technology currently on the market is still immature, and most of them are various water-based resins, whose adhesion and water washability are far from meeting production needs. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention provides a TPU hot-melt powder modified waterborne polyurethane resin and a preparation method thereof, which has the advantages of strong product adhesion and improved water washability, and the comprehensive performance of the product is improved.

[0007] (II) Technical solution

[0008] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a TPU hot-melt powder modified waterborne polyurethane resin, comprising the following raw materials in parts by weight: 30-55 parts of deionized water, 8-30 parts of diisocyanate, 22-45 parts of oligomer polyol, 0.1-3.2 parts of chain extender, 0.1-3.2 parts of hydrophilic chain extender, 3-35 parts of TPU hot-melt powder, 0.2-0.6 parts of salt-forming agent, and 0.06-0.5 parts of catalyst. The particle size of the TPU hot-melt powder is ≤85um, the melting point range is 93-107°C, and the thermal bonding temperature is 145-165°C.

[0009] Preferably, the type of diisocyanate is toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate and isophorone diisocyanate. Isocyanate groups can react with active hydrogen compounds, and the reaction mechanism is caused by the attack of the nucleophilic center in the active hydrogen compound molecule on the carbon atom of the NCO group. The electron cloud density on the carbon atom in the isocyanate group is the lowest, with a strong positive charge, which is an electrophilic center and is easily attacked by nucleophilic reagents. The electron cloud density on oxygen atoms and nitrogen atoms is higher, with a strong negative charge, and the electronegativity of oxygen atoms is the largest, which is a nucleophilic center and can attract hydrogen atoms to generate hydroxyls, but the hydroxyls on unsaturated carbon atoms are unstable and easily rearranged into carbamates.

[0010] Preferably, the chain extender containing anions includes two categories: carboxyl-containing and sulfonic acid-containing. The sulfonic acid-containing chain extenders include sodium ethylenediamine ethanesulfonate, sodium N,N-(2-hydroxyethyl)-2-aminoethanesulfonate (BES sodium salt), and 1,4-butanediol-2-sulfonate. The cationic chain extender is mainly methyldiethanolamine. The hydrophilic chain extender is dimethylolpropionic acid. Chain extenders also need to be added in the preparation of water-based polyurethane. Chain extenders can make polyurethane form linear or bulk macromolecules, improve the strength and medium resistance of polyurethane, and although amine chain extenders have high reactivity, they are relatively toxic.

[0011] Preferably, the oligomer polyol adopts polyester diol, and its types include polycarbonate diol, polycaprolactone diol, polybutadiene diol, acrylate polyol, polyethylene adipate diol and / or polyneopentyl adipate diol. In the preparation of waterborne polyurethane, oligomer polyol generally uses polyether diol and polyester diol. Polyether polyurethane still has good hydrolysis stability even in the presence of acid and alkali, because of the presence of ether bond, the hydrophilicity of ether bond is better than that of ester bond. Polyether polyurethane has the advantages of low softening temperature, good low temperature resistance, good toughness and elongation.

[0012] Preferably, the salt-forming agent is triethylamine, NaOH, diethanolamine or diisopropanolamine. In theory, any acid or alkaline substance with a certain strength can be used as a salt-forming agent for preparing waterborne polyurethane. However, the selection of different salt-forming agents has a great influence on the performance of the product, and the salt-forming agent has a regulating effect on the viscosity and color of the product. The main conditions for selecting the salt-forming agent are: making the emulsion stable, small in color change, good in appearance, and economical and easy to obtain. For cationic waterborne polyurethane, most cationic waterborne polyurethanes are prepared by introducing tertiary amines into polyurethane macromolecules, so they all contain tertiary amines on their molecules. In theory, any reagent that can react with the tertiary amine on the molecule to undergo quaternization reaction meets the conditions for being used as a salt-forming agent for cationic waterborne polyurethane. Hydrohalic acid and organic halide are mostly used as salt-forming agents for preparing cationic waterborne polyurethane. For anionic polyurethane, any alkaline substance that can react with anionic groups to undergo neutralization reaction meets the conditions for being used as a salt-forming agent for preparing anionic polyurethane.

[0013] Preferably, the method for preparing the TPU hot melt powder modified waterborne polyurethane resin comprises the following steps:

[0014] S1: First, dehydrate the TPU hot melt powder and oligomer polyol at high temperature for 1-3 hours, then add diisocyanate when the temperature drops to a certain temperature, and heat up and stir.

[0015] S2: adding a small molecule chain extender, a hydrophilic chain extender and a catalyst in order to react, and adjusting the viscosity of the reaction system with acetone during the whole reaction process to obtain a polyurethane prepolymer.

[0016] S3: The polyurethane prepolymer obtained by the reaction is transferred into an emulsifying device. When the temperature is 20-50°C, a salt-forming agent is added into the emulsifying device. After the reaction lasts for 1-3 minutes, deionized water is added and stirred rapidly.

[0017] S4: The acetone-containing emulsion prepared in the third step is transferred to a deacetone removal device, the temperature is controlled at 32-60° C., and the acetone is removed under vacuum conditions to obtain an aqueous polyurethane emulsion.

[0018] (III) Beneficial effects

[0019] Compared with the prior art, the present invention provides a method for preparing a TPU hot-melt powder modified waterborne polyurethane resin, which has the following beneficial effects:

[0020] 1. The TPU hot melt powder modified waterborne polyurethane resin and its preparation method, by adding medium and high temperature TPU hot melt powder to prepare the modified waterborne polyurethane resin, increases the adhesion of the product and also improves the water washability, thereby improving the comprehensive performance of the product to meet industrial needs.

[0021] 2. The TPU hot-melt powder modified water-based polyurethane resin and its preparation method can function better in a dark and humid environment due to its relatively high humidity, and its adhesion is more durable. In addition, its gloss is not strong, and after use, it will appear that there are no major traces of adhesion. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Embodiment 1:

[0024] The invention provides a TPU hot-melt powder modified waterborne polyurethane resin, comprising the following raw materials in parts by weight: 30 parts of deionized water, 28 parts of diisocyanate, 22 parts of oligomer polyol, 0.64 parts of chain extender, 0.1 parts of hydrophilic chain extender, 19 parts of TPU hot-melt powder, 0.2 parts of salt-forming agent, and 0.06 parts of catalyst. The particle size of the TPU hot-melt powder is 80 μm, the melting point range is 93° C., and the thermal bonding temperature is 145° C.

[0025] A method for preparing a TPU hot-melt powder modified waterborne polyurethane resin comprises the following steps:

[0026] S1: First, dehydrate the TPU hot melt powder and oligomer polyol at 115°C for 1.2 hours, then add diisocyanate when the temperature is lowered to 71°C, and heat to 86°C for stirring reaction for 1.3 hours.

[0027] S2: Then, a small molecule chain extender, a hydrophilic chain extender and a catalyst were added in order to react. The temperature was controlled at 58° C. and the reaction time was 4.8 h. During the whole reaction process, acetone was used to adjust the viscosity of the reaction system to obtain a polyurethane prepolymer.

[0028] S3: The polyurethane prepolymer obtained by the reaction is transferred into an emulsifying device. When the temperature is 30°C, a salt-forming agent is added into the emulsifying device. After the reaction lasts for 1.5 minutes, deionized water is added and stirred rapidly.

[0029] S4: The acetone-containing emulsion prepared in the third step is transferred to a deacetone removal device, the temperature is controlled at 40° C., and the acetone is removed under vacuum conditions to obtain an aqueous polyurethane emulsion.

[0030] Embodiment 2:

[0031] The invention provides a TPU hot-melt powder modified waterborne polyurethane resin, comprising the following raw materials in parts by weight: 40 parts of deionized water, 22 parts of diisocyanate, 31 parts of oligomer polyol, 0.64 parts of chain extender, 0.1 parts of hydrophilic chain extender, 6 parts of TPU hot-melt powder, 0.2 parts of salt-forming agent, and 0.06 parts of catalyst. The particle size of the TPU hot-melt powder is 75 μm, the melting point range is 96° C., and the thermal bonding temperature is 150° C.

[0032] A method for preparing a TPU hot-melt powder modified waterborne polyurethane resin comprises the following steps:

[0033] S1: First, dehydrate the TPU hot melt powder and oligomer polyol at 117°C for 1.5 hours, then add diisocyanate when the temperature is lowered to 65°C, and heat to 90°C for stirring reaction for 1.6 hours.

[0034] S2: Then, a small molecule chain extender, a hydrophilic chain extender and a catalyst are added in order to react. The temperature is controlled at 60° C. and the reaction time is 5 hours. During the whole reaction process, acetone is used to adjust the viscosity of the reaction system to obtain a polyurethane prepolymer.

[0035] S3: The polyurethane prepolymer obtained by the reaction is transferred into an emulsifying device. When the temperature is 34°C, a salt-forming agent is added into the emulsifying device. After the reaction lasts for 1.7 minutes, deionized water is added and stirred rapidly.

[0036] S4: The acetone-containing emulsion prepared in the third step is transferred to a deacetone removal device, the temperature is controlled at 45° C., and the acetone is removed under vacuum conditions to obtain an aqueous polyurethane emulsion.

[0037] Embodiment three:

[0038] The invention provides a TPU hot-melt powder modified waterborne polyurethane resin, which comprises the following raw materials in parts by weight: 50 parts of deionized water, 15 parts of diisocyanate, 30 parts of oligomer polyol, 0.2 parts of chain extender, 0.1 parts of hydrophilic chain extender, 4 parts of TPU hot-melt powder, 0.3 parts of salt-forming agent and 0.4 parts of catalyst. The particle size of the TPU hot-melt powder is 70 μm, the melting point range is 100° C. and the thermal bonding temperature is 155° C.

[0039] A method for preparing a TPU hot-melt powder modified waterborne polyurethane resin comprises the following steps:

[0040] S1: First, dehydrate the TPU hot melt powder and oligomer polyol at 119°C for 1.8 hours, then add diisocyanate when the temperature is lowered to 63°C, and heat to 95°C for stirring reaction for 1.8 hours.

[0041] S2: Then, a small molecule chain extender, a hydrophilic chain extender and a catalyst were added in order to react. The temperature was controlled at 65° C. and the reaction time was 5.3 h. During the whole reaction process, acetone was used to adjust the viscosity of the reaction system to obtain a polyurethane prepolymer.

[0042] S3: The polyurethane prepolymer obtained by the reaction is transferred into an emulsifying device. When the temperature is 38°C, a salt-forming agent is added into the emulsifying device. After the reaction lasts for 1.9 minutes, deionized water is added and stirred rapidly.

[0043] S4: The acetone-containing emulsion prepared in the third step is transferred to a deacetone removal device, the temperature is controlled at 50° C., and the acetone is removed under vacuum conditions to obtain an aqueous polyurethane emulsion.

[0044] Embodiment 4:

[0045] The invention provides a TPU hot-melt powder modified waterborne polyurethane resin, comprising the following raw materials in parts by weight: 60 parts of deionized water, 15 parts of diisocyanate, 15 parts of oligomer polyol, 2 parts of chain extender, 2.5 parts of hydrophilic chain extender, 4.5 parts of TPU hot-melt powder, 0.5 parts of salt-forming agent, and 0.5 parts of catalyst. The particle size of the TPU hot-melt powder is 65 μm, the melting point range is 105° C., and the thermal bonding temperature is 165° C.

[0046] A method for preparing a TPU hot melt powder modified waterborne polyurethane resin comprises the following steps:

[0047] S1: First, dehydrate the TPU hot melt powder and oligomer polyol at 125°C for 2.5 hours, then add diisocyanate when the temperature is lowered to 60°C, and heat to 100°C for stirring reaction for 2.5 hours.

[0048] S2: Then, a small molecule chain extender, a hydrophilic chain extender and a catalyst are added in order to react. The temperature is controlled at 70° C. and the reaction time is 6 hours. During the whole reaction process, acetone is used to adjust the viscosity of the reaction system to obtain a polyurethane prepolymer.

[0049] S3: The polyurethane prepolymer obtained by the reaction is transferred into an emulsifying device. When the temperature is 45°C, a salt-forming agent is added into the emulsifying device. After the reaction lasts for 2.5 minutes, deionized water is added and stirred rapidly.

[0050] S4: The acetone-containing emulsion prepared in the third step is transferred to a deacetone removal device, the temperature is controlled at 60° C., and the acetone is removed under vacuum conditions to obtain an aqueous polyurethane emulsion.

[0051] In summary: different amounts of raw materials were added according to the methods in Example 1, Example 2, Example 3 and Example 4 for reaction. The results showed that the effect of preparing TPU hot-melt powder modified waterborne polyurethane resin according to the amounts of raw materials in Example 2 and Example 4 was the best.

[0052] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A TPU hot melt powder modified waterborne polyurethane resin, characterized in that: The invention comprises the following raw materials in parts by weight: 30-55 parts of deionized water, 8-30 parts of diisocyanate, 22-45 parts of oligomer polyol, 0.1-3.2 parts of chain extender, 0.1-3.2 parts of hydrophilic chain extender, 3-35 parts of TPU hot melt powder, 0.2-0.6 parts of salt-forming agent and 0.06-0.5 parts of catalyst; the particle size of the TPU hot melt powder is ≤85um, the melting point range is 93-107°C and the thermal bonding temperature is 145-165°C.

2. A TPU hot melt powder modified waterborne polyurethane resin according to claim 1, characterized in that: The types of the diisocyanates are toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate and isophorone diisocyanate.

3. A TPU hot melt powder modified waterborne polyurethane resin according to claim 1, characterized in that: The chain extenders containing anions include two categories: carboxyl-containing and sulfonic acid-containing. The sulfonic acid-containing chain extenders include sodium ethylenediamine ethanesulfonate, sodium N,N-(2-hydroxyethyl)-2-aminoethanesulfonate (BES sodium salt), and sodium 1,4-butanediol-2-sulfonate. The cationic chain extenders are mainly methyldiethanolamine. The hydrophilic chain extender is dihydroxymethylpropionic acid.

4. The TPU hot melt powder modified waterborne polyurethane resin according to claim 1, characterized in that: The oligomer polyol is a polyester diol, and its types include polycarbonate diol, polycaprolactone diol, polybutadiene diol, acrylate polyol, polyethylene adipate diol and / or polyneopentyl adipate diol.

5. The TPU hot melt powder modified waterborne polyurethane resin according to claim 1, characterized in that: The salt-forming agent is triethylamine, NaOH, diethanolamine or diisopropanolamine.

6. A TPU hot melt powder modified waterborne polyurethane resin according to any one of claims 1 to 5, characterized in that: The preparation method of the TPU hot melt powder modified waterborne polyurethane resin specifically comprises the following steps: S1: First, dehydrate TPU hot melt powder and oligomer polyol at high temperature for 1-3 hours, then add diisocyanate when the temperature drops to a certain temperature, and heat up and stir; S2: adding a small molecule chain extender, a hydrophilic chain extender and a catalyst in order to react, and adjusting the viscosity of the reaction system with acetone during the whole reaction process to obtain a polyurethane prepolymer; S3: The polyurethane prepolymer obtained by the reaction is transferred into an emulsifier. When the temperature is 20-50°C, a salt-forming agent is added into the emulsifier. After the reaction lasts for 1-3 minutes, deionized water is added and stirred rapidly. S4: The acetone-containing emulsion prepared in the third step is transferred to a deacetone removal device, the temperature is controlled at 32-60° C., and the acetone is removed under vacuum conditions to obtain an aqueous polyurethane emulsion.