Carbon fiber reinforced polyurethane rubber synchronous belt and preparation method thereof

By using carbon fiber reinforced polyurethane rubber design in the synchronization belt, combined with specific raw materials and process processing, a multiple interpenetrating network structure is formed, which solves the shortcomings of the synchronization belt in terms of cold resistance, heat aging resistance and wear resistance, and significantly improves the Performance and stability.

CN118994891APending Publication Date: 2024-11-22NINGBO FULONG SYNCHRONOUS BELT

Patent Information

Application Number
CN202411487661.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing synchronous belts have shortcomings in terms of cold resistance, heat aging resistance, flame retardancy and wear resistance, resulting in safety hazards and poor performance in some application environments.

Method used

The design of carbon fiber reinforced polyurethane rubber synchronous belt is adopted, including the main glue layer, the surface elastic buffer layer modified carbon fiber skeleton layer and the cloth cladding layer. Through specific raw material combinations and process processing, multiple interpenetrating network structures are formed to improve performance.

Benefits of technology

It significantly improves the environmentally friendly flame retardant, mechanical and mechanical properties, heat aging resistance and cold resistance of the synchronization belt, extends the service life and improves stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a carbon fiber reinforced polyurethane rubber synchronous belt and a preparation method thereof, and relates to the technical field of synchronous belts, the carbon fiber reinforced polyurethane rubber synchronous belt sequentially comprises a main body rubber layer, a surface elastic buffer layer modified carbon fiber skeleton layer and a wrapping cloth layer from top to bottom; the main body rubber layer is prepared from the following raw materials: polyether mixed polyurethane rubber, a thermoplastic polyester elastomer, 1, 3-bis (oxiranyl methyl)-5-(2-propenyl)-1, 3, 5-triazine-2, 4, 6 (1H, 3H, 5H)-triketone, 3, 3 '-diamino-4, 4'-difluorodiphenyl sulfone, (3, 3 '-bis (oxiranyl methyl)-5-(2-propenyl)-1, 3, 5-triazine-2, 4, 6 (1H, 3H, 5H)-triketone, 3, 3'-bis (oxiranyl methyl)-5-(2-propenyl)- The anti-scorching coating is prepared from 2, 6-diamino-9-acridinyl) boric acid, 2-acrylamido-2-methylpropanesulfonic acid, inorganic filler, a coupling agent, a vulcanizing agent, phosphorus pentoxide, polyphosphoric acid, an anti-aging agent, stearic acid and an anti-scorching agent. The carbon fiber reinforced polyurethane rubber synchronous belt is environment-friendly, good in flame retardance, excellent in mechanical property and excellent in heat aging resistance, cold resistance and wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of synchronous belts, and in particular to a carbon fiber reinforced polyurethane rubber synchronous belt and a preparation method thereof. Background Art

[0002] Synchronous belt is a new type of conveyor belt developed by combining the advantages of belt drive, chain drive and gear drive. Compared with chain and gear drive, synchronous belt drive has the advantages of smooth transmission, small impact, no lubrication, no pollution, low noise, high transmission efficiency, accurate transmission ratio, wide transmission ratio range, energy saving, etc. It is widely used in textile machinery, automobiles, tobacco machinery, food machinery, light industry, chemical industry, computers and general machinery.

[0003] The main rubber materials of traditional synchronous belts are polyurethane rubber, chloroprene rubber and nitrile rubber. The synchronous belts made of these rubber materials have more or less defects such as poor cold resistance, insufficient strength, insufficient heat aging resistance and flame retardancy, and the mechanical properties and environmental protection flame retardancy need to be further improved. There are safety hazards when used in some special occasions.

[0004] Carbon fiber has the advantages of excellent specific strength and stiffness, low thermal expansion, high modulus, high wear resistance, corrosion resistance, etc., and is widely used in aviation, transportation, batteries, sporting goods and other fields. In recent years, in order to improve the performance of synchronous belts, the reinforcement skeleton of synchronous belts is mostly composed of carbon fiber twisted ropes, but the surface of carbon fiber is chemically inert, amphiphobic, and smooth, and it is poorly impregnated with rubber resins and the like and it is difficult to form a strong interaction, resulting in unsatisfactory interface performance between the rope and the rubber matrix, and ultimately causing the performance of the synchronous belt to fail to meet expectations.

[0005] In order to solve the above problems, the Chinese invention patent with the authorization announcement number CN115679711B discloses a multifunctional carbon fiber reinforced polyurethane rubber synchronous toothed belt and a preparation method, wherein the synchronous toothed belt comprises a back belt surface rubber functional layer, a polyurethane rubber base belt layer, a carbon fiber skeleton layer, belt teeth and tooth surfaces arranged in sequence; the back belt surface rubber functional layer is any one of polyurethane rubber, natural rubber, nitrile rubber, EPDM rubber and silicone rubber. The carbon fiber skeleton layer accounts for 5-25% of the thickness of the back belt surface rubber layer; the carbon fiber skeleton layer is a carbon fiber fabric woven from different tow carbon fibers; the carbon fiber fabric is subjected to surface treatment and sizing treatment in sequence; the sizing rate of the carbon fiber fabric is 0.5-0.8%, the surface tension of the sizing agent is 43-47mN / m, and the viscosity is 1.5-2.5cp. The synchronous toothed belt prepared by this invention has high strength, good wear resistance, low elongation and good dimensional stability, which solves the problem that some synchronous belts are prone to deformation and poor creep resistance during long-term use. It is suitable for different application environments with high requirements for product dimensional accuracy, heavy load and high requirements for wear resistance. However, its cold resistance, wear resistance, flame retardancy and heat aging resistance still need to be further improved.

[0006] It can be seen that the development of a carbon fiber reinforced polyurethane rubber synchronous belt with good environmental protection and flame retardancy, good mechanical properties, excellent heat aging resistance, cold resistance and wear resistance and its preparation method meets market demand, has broad market value and application prospects, and is of great significance to promoting the development of the synchronous belt field. Summary of the invention

[0007] In view of this, the technical problem to be solved by the present invention is to provide a carbon fiber reinforced polyurethane rubber synchronous belt with good environmental protection and flame retardancy, good mechanical properties, excellent heat aging resistance, cold resistance and wear resistance, and a preparation method thereof.

[0008] The present invention provides a carbon fiber reinforced polyurethane rubber synchronous belt, which comprises, from top to bottom, a main body rubber layer, a carbon fiber skeleton layer modified by a surface elastic buffer layer, and a cloth layer; the main body rubber layer is made of the following raw materials in parts by weight: 60-70 parts of polyether mixed polyurethane rubber, 10-20 parts of thermoplastic polyester elastomer, 1,3-bis(oxiranylmethyl)-5-(2-propylene)-1,3,5-triazine-2,4,6(1H,3H, 5H)-trione 3-5 parts, 3,3'-diamino-4,4'-difluorodiphenyl sulfone 1-3 parts, (3,6-diamino-9-acridinyl)boric acid 1-3 parts, 2-acrylamido-2-methylpropanesulfonic acid 2-4 parts, inorganic filler 15-25 parts, coupling agent 3-5 parts, vulcanizing agent 2-4 parts, phosphorus pentoxide 1-3 parts, polyphosphoric acid 0.5-0.8 parts, antioxidant 1-3 parts, stearic acid 1-3 parts, scorch retarder 0.3-0.5 parts.

[0009] Preferably, the polyether mixing type polyurethane rubber is a rubber with an unsaturated structure synthesized by using polyether polyol and 4,4'-diphenylmethane diisocyanate (MDI) as main raw materials, and the brand is UR101.

[0010] Preferably, the thermoplastic polyester elastomer is Riteflex® TPC-ET thermoplastic polyester elastomer.

[0011] Preferably, the inorganic filler is a mixture of white carbon black and carbon nanofibers in a mass ratio of (1-3):1; the particle size of the white carbon black is 1000-1500 mesh; the average diameter of the carbon nanofibers is 50-100nm, and the aspect ratio is (20-30):1.

[0012] Preferably, the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.

[0013] Preferably, the vulcanizing agent is a mixture of dipentamethylenethiuram tetrasulfide, vulcanizing agent bis-25, benzoyl peroxide, and dicumyl peroxide in a mass ratio of 1:(0.3-0.7):0.5:(0.8-1.2).

[0014] Preferably, the antioxidant is at least one of antioxidant NBC and antioxidant BLE.

[0015] Preferably, the anti-scorch agent is anti-scorch agent CTP.

[0016] Preferably, the surface elastic buffer layer is made of the following raw materials in parts by weight: 50-70 parts of epoxidized natural rubber, 20-30 parts of amino-containing hyperbranched polyurethane, 3-5 parts of trirosin acid glycerol, 1-3 parts of bis(3-aminophenyl)3,5-bis(trifluoromethyl)phenylphosphine oxide, and 10-20 parts of toluene.

[0017] Preferably, the epoxidation rate of the epoxidized natural rubber is 25%, which is provided by the Chinese Academy of Tropical Agricultural Sciences.

[0018] Preferably, there is no special requirement for the source of the amino-containing hyperbranched polyurethane. In one embodiment of the present invention, the amino-containing hyperbranched polyurethane is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN104693405B.

[0019] Preferably, the thickness of the main rubber layer is 8-12 mm, the thickness of the surface elastic buffer layer is 1-2 mm, the thickness of the carbon fiber skeleton modified by the surface elastic buffer layer is 4-6 mm; and the carbon fiber skeleton is made of carbon fiber cords.

[0020] Another object of the present invention is to provide a method for preparing the carbon fiber reinforced polyurethane rubber synchronous belt, comprising the following steps: Step S1, preparation of a carbon fiber skeleton layer modified with a surface elastic buffer layer: after uniformly mixing the raw materials of the surface elastic buffer layer, adding them into a glue machine, uniformly dispersing them by ultrasonic-assisted stirring to obtain glue, then immersing a carbon fiber skeleton made of carbon fiber cords in the glue, taking it out and curing it at 110-120° C. for 1-2 hours to obtain a carbon fiber skeleton layer modified with a surface elastic buffer layer; Step S2, preparation of the main rubber layer: putting the polyether mixing type polyurethane rubber and the thermoplastic polyester elastomer into an open mill for mixing, alternately adding other raw materials, and mixing evenly to obtain the main rubber layer; Step S3, wrapping and laminating: wrapping and laminating the main adhesive layer and the cloth layer on the carbon fiber skeleton layer modified by the surface elastic buffer layer in the order of main adhesive layer, carbon fiber skeleton layer modified by the surface elastic buffer layer and cloth layer from top to bottom, and then placing it in a synchronous belt mold for pressing and vulcanization, and cooling to room temperature to obtain a carbon fiber reinforced polyurethane rubber synchronous belt.

[0021] Preferably, in step S3, the vulcanization temperature is 170-190° C., the vulcanization pressure is 8-12 MPa, and the vulcanization time is 30-40 min.

[0022] Due to the application of the above technical solution, the present invention has the following beneficial effects: (1) The method for preparing the carbon fiber reinforced polyurethane rubber synchronous belt disclosed in the present invention has a simple process, convenient operation and control, high preparation efficiency and finished product qualification rate, is suitable for continuous large-scale production, and has a high value for promotion and application.

[0023] (2) The carbon fiber reinforced polyurethane rubber synchronous belt disclosed in the present invention comprises, from top to bottom, a main rubber layer, a carbon fiber skeleton layer modified by a surface elastic buffer layer, and a cloth layer; such a structural design can effectively improve the stability of the synchronous belt, prevent delamination, and extend its service life; the provision of the elastic buffer layer can improve the compatibility and bonding performance between the carbon fiber skeleton and the cloth layer and the main rubber layer, improve elasticity, and further improve its use effect and extend its service life.

[0024] (3) The carbon fiber reinforced polyurethane rubber synchronous belt disclosed in the present invention, the main rubber layer is made of the following raw materials in parts by weight: 60-70 parts of polyether mixed polyurethane rubber, 10-20 parts of thermoplastic polyester elastomer, 3-5 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, and 3,3'- 1-3 parts of diamino-4,4'-difluorodiphenyl sulfone, 1-3 parts of (3,6-diamino-9-acridinyl)boric acid, 2-4 parts of 2-acrylamido-2-methylpropanesulfonic acid, 15-25 parts of inorganic filler, 3-5 parts of coupling agent, 2-4 parts of vulcanizing agent, 1-3 parts of phosphorus pentoxide, 0.5-0.8 parts of polyphosphoric acid, 1-3 parts of antioxidant, 1-3 parts of stearic acid, and 0.3-0.5 parts of scorch retarder. The polyether mixed polyurethane rubber and thermoplastic polyester elastomer are blended as the base material, and the advantages of each are combined to make the synchronous belt have good environmental protection and flame retardancy, good mechanical properties, excellent heat aging resistance, cold resistance and wear resistance; through the mutual cooperation between the components of the main rubber layer preparation raw materials, polyurethane rubber, thermoplastic polyester elastomer, triazone, difluorodiphenyl sulfone, acridinyl boric acid structure are introduced into the main rubber layer structure at the same time. These structures make the environmental protection and flame retardancy of the manufactured products better, better mechanical properties, better heat aging resistance, cold resistance and wear resistance under the multiple effects of electronic effect, steric effect and conjugation effect. The raw materials containing amino groups can undergo epoxy ring-opening reaction with the raw materials containing epoxy groups, and the raw materials containing unsaturated olefin bonds can undergo copolymerization reaction. The raw materials containing sulfonic acid groups can react chemically with the raw materials containing benzene rings under the catalytic action of phosphorus pentoxide and polyphosphoric acid to form a multiple interpenetrating network structure, further improving the above properties.

[0025] (4) The carbon fiber reinforced polyurethane rubber synchronous belt disclosed in the present invention, the surface elastic buffer layer is made of the following raw materials by weight: 50-70 parts of epoxidized natural rubber, 20-30 parts of hyperbranched polyurethane containing amino groups, 3-5 parts of trirosin acid glycerol, 1-3 parts of bis(3-aminophenyl)3,5-bis(trifluoromethyl)phenylphosphine oxide, and 10-20 parts of toluene. Through the mutual cooperation between the components, not only the elasticity can be improved, but also the bonding performance between the layers of the synchronous belt can be effectively improved, thereby improving the performance stability of the synchronous belt and effectively extending its service life. DETAILED DESCRIPTION

[0026] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.

[0027] The cloth layer in each embodiment of the present invention is a nylon cloth layer. Example 1

[0028] A carbon fiber reinforced polyurethane rubber synchronous belt comprises, from top to bottom, a main rubber layer, a carbon fiber skeleton layer modified by a surface elastic buffer layer, and a cloth layer; the main rubber layer is made of the following raw materials in parts by weight: 60 parts of polyether mixed polyurethane rubber, 10 parts of thermoplastic polyester elastomer, 3 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1 part of 3,3'-diamino-4,4'-difluorodiphenyl sulfone, 1 part of (3,6-diamino-9-acridinyl)boric acid, 2 parts of 2-acrylamido-2-methylpropanesulfonic acid, 15 parts of inorganic filler, 3 parts of coupling agent, 2 parts of vulcanizing agent, 1 part of phosphorus pentoxide, 0.5 parts of polyphosphoric acid, 1 part of antioxidant, 1 part of stearic acid, and 0.3 parts of scorch retarder.

[0029] The polyether compounded polyurethane rubber is a rubber with an unsaturated structure synthesized with polyether polyol and 4,4'-diphenylmethane diisocyanate (MDI) as the main raw materials, and its brand is UR101; the thermoplastic polyester elastomer is Riteflex® TPC-ET thermoplastic polyester elastomer; the inorganic filler is a mixture of white carbon black and carbon nanofiber in a mass ratio of 1:1; the particle size of the white carbon black is 1000 mesh; the average diameter of the carbon nanofiber is 50nm, and the aspect ratio is 20:1.

[0030] The coupling agent is silane coupling agent KH550; the vulcanizing agent is a mixture of dipentamethylenethiuram tetrasulfide, vulcanizing agent bis 25, benzoyl peroxide, and diisopropylbenzene peroxide in a mass ratio of 1:0.3:0.5:0.8; the antioxidant is antioxidant NBC; and the anti-scorch agent is anti-scorch agent CTP.

[0031] The surface elastic buffer layer is made of the following raw materials in parts by weight: 50 parts of epoxidized natural rubber, 20 parts of hyperbranched polyurethane containing amino groups, 3 parts of trirosin acid glycerol, 1 part of bis(3-aminophenyl)3,5-bis(trifluoromethyl)phenylphosphine oxide, and 10 parts of toluene; the epoxidation rate of the epoxidized natural rubber is 25%, which is provided by the Chinese Academy of Tropical Agricultural Sciences; the hyperbranched polyurethane containing amino groups is made according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN104693405B.

[0032] The thickness of the main rubber layer is 12 mm, the thickness of the surface elastic buffer layer is 1 mm, the thickness of the carbon fiber skeleton modified by the surface elastic buffer layer is 4 mm; and the carbon fiber skeleton is made of carbon fiber cords.

[0033] A method for preparing the carbon fiber reinforced polyurethane rubber synchronous belt comprises the following steps: Step S1, preparation of a carbon fiber skeleton layer modified with a surface elastic buffer layer: after uniformly mixing the raw materials of the surface elastic buffer layer, adding them into a glue machine, uniformly dispersing them by ultrasonic-assisted stirring to obtain glue, then immersing a carbon fiber skeleton made of carbon fiber cords in the glue, taking it out and curing it at 110° C. for 1 hour to obtain a carbon fiber skeleton layer modified with a surface elastic buffer layer; Step S2, preparation of the main rubber layer: putting the polyether mixing type polyurethane rubber and the thermoplastic polyester elastomer into an open mill for mixing, alternately adding other raw materials, and mixing evenly to obtain the main rubber layer; Step S3, wrapping and laminating: wrapping and laminating the main adhesive layer and the cloth layer on the carbon fiber skeleton layer modified by the surface elastic buffer layer in the order of the main adhesive layer, the carbon fiber skeleton layer modified by the surface elastic buffer layer and the cloth layer from top to bottom, and then placing it in a synchronous belt mold for pressing and vulcanization, and cooling to room temperature to obtain a carbon fiber reinforced polyurethane rubber synchronous belt; the vulcanization temperature is 170°C, the vulcanization pressure is 8MPa, and the vulcanization time is 30min. Example 2

[0034] A carbon fiber reinforced polyurethane rubber synchronous belt, which comprises, from top to bottom, a main rubber layer, a carbon fiber skeleton layer modified by a surface elastic buffer layer, and a cloth layer; the main rubber layer is made of the following raw materials in parts by weight: 63 parts of polyether mixed polyurethane rubber, 12 parts of thermoplastic polyester elastomer, 1,3-bis(oxiranylmethyl)-5-(2-propylene)-1,3,5-triazine-2,4,6(1H,3H, 5H)-trione 3.5 parts, 3,3'-diamino-4,4'-difluorodiphenyl sulfone 1.5 parts, (3,6-diamino-9-acridinyl)boric acid 1.5 parts, 2-acrylamido-2-methylpropanesulfonic acid 2.5 parts, inorganic filler 17 parts, coupling agent 3.5 parts, vulcanizing agent 2.5 parts, phosphorus pentoxide 1.5 parts, polyphosphoric acid 0.6 parts, antioxidant 1.5 parts, stearic acid 1.5 parts, scorch retarder 0.35 parts.

[0035] The polyether compounded polyurethane rubber is a rubber with an unsaturated structure synthesized with polyether polyol and 4,4'-diphenylmethane diisocyanate (MDI) as the main raw materials, and its brand is UR101; the thermoplastic polyester elastomer is Riteflex® TPC-ET thermoplastic polyester elastomer; the inorganic filler is a mixture of white carbon black and carbon nanofiber in a mass ratio of 1.5:1; the particle size of the white carbon black is 1200 mesh; the average diameter of the carbon nanofiber is 70nm, and the aspect ratio is 23:1.

[0036] The coupling agent is silane coupling agent KH560; the vulcanizing agent is a mixture of dipentamethylenethiuram tetrasulfide, vulcanizing agent bis 25, benzoyl peroxide, and diisopropylbenzene peroxide in a mass ratio of 1:0.4:0.5:0.9; the antioxidant is antioxidant BLE; and the anti-scorch agent is anti-scorch agent CTP.

[0037] The surface elastic buffer layer is made of the following raw materials in parts by weight: 55 parts of epoxidized natural rubber, 23 parts of hyperbranched polyurethane containing amino groups, 3.5 parts of trirosin acid glycerol, 1.5 parts of bis(3-aminophenyl)3,5-bis(trifluoromethyl)phenylphosphine oxide, and 13 parts of toluene; the epoxidation rate of the epoxidized natural rubber is 25%, which is provided by the Chinese Academy of Tropical Agricultural Sciences; the hyperbranched polyurethane containing amino groups is made according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN104693405B.

[0038] The thickness of the main rubber layer is 12 mm, the thickness of the surface elastic buffer layer is 1 mm, the thickness of the carbon fiber skeleton modified by the surface elastic buffer layer is 4 mm; and the carbon fiber skeleton is made of carbon fiber cords.

[0039] The method for preparing the carbon fiber reinforced polyurethane rubber synchronous belt comprises the following steps: Step S1, preparation of a carbon fiber skeleton layer modified with a surface elastic buffer layer: after uniformly mixing the raw materials of the surface elastic buffer layer, adding them into a glue machine, uniformly dispersing them by ultrasonic-assisted stirring to obtain glue, then immersing a carbon fiber skeleton made of carbon fiber cords in the glue, taking it out and curing it at 113° C. for 1.2 hours to obtain a carbon fiber skeleton layer modified with a surface elastic buffer layer; Step S2, preparation of the main rubber layer: putting the polyether mixing type polyurethane rubber and the thermoplastic polyester elastomer into an open mill for mixing, alternately adding other raw materials, and mixing evenly to obtain the main rubber layer; Step S3, wrapping and laminating: wrapping and laminating the main adhesive layer and the cloth layer on the carbon fiber skeleton layer modified by the surface elastic buffer layer in the order of the main adhesive layer, the carbon fiber skeleton layer modified by the surface elastic buffer layer and the cloth layer from top to bottom, and then placing it in a synchronous belt mold for pressing and vulcanization, and cooling to room temperature to obtain a carbon fiber reinforced polyurethane rubber synchronous belt; the vulcanization temperature is 175°C, the vulcanization pressure is 9MPa, and the vulcanization time is 33min. Example 3

[0040] A carbon fiber reinforced polyurethane rubber synchronous belt comprises, from top to bottom, a main rubber layer, a carbon fiber skeleton layer modified by a surface elastic buffer layer, and a cloth layer; the main rubber layer is made of the following raw materials in parts by weight: 65 parts of polyether mixed polyurethane rubber, 15 parts of thermoplastic polyester elastomer, 4 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2 parts of 3,3'-diamino-4,4'-difluorodiphenyl sulfone, 2 parts of (3,6-diamino-9-acridinyl)boric acid, 3 parts of 2-acrylamido-2-methylpropanesulfonic acid, 20 parts of inorganic filler, 4 parts of coupling agent, 3 parts of vulcanizing agent, 2 parts of phosphorus pentoxide, 0.65 parts of polyphosphoric acid, 2 parts of antioxidant, 2 parts of stearic acid, and 0.4 parts of scorch retarder.

[0041] The polyether compounded polyurethane rubber is a rubber with an unsaturated structure synthesized by using polyether polyol and 4,4'-diphenylmethane diisocyanate (MDI) as main raw materials, and its brand is UR101; the thermoplastic polyester elastomer is Riteflex® TPC-ET thermoplastic polyester elastomer; the inorganic filler is a mixture of white carbon black and carbon nanofiber in a mass ratio of 2:1; the particle size of the white carbon black is 1300 mesh; the average diameter of the carbon nanofiber is 80nm, and the aspect ratio is 25:1; the coupling agent is a silane coupling agent KH570; the vulcanizing agent is a mixture of tetrasulfide dipentamethylenethiuram, vulcanizing agent di-25, benzoyl peroxide, and diisopropylbenzene peroxide in a mass ratio of 1:0.5:0.5:1; the antioxidant is antioxidant NBC; and the anti-scorch agent is anti-scorch agent CTP.

[0042] The surface elastic buffer layer is made of the following raw materials in parts by weight: 60 parts of epoxidized natural rubber, 25 parts of hyperbranched polyurethane containing amino groups, 4 parts of trirosin acid glycerol, 2 parts of bis(3-aminophenyl)3,5-bis(trifluoromethyl)phenylphosphine oxide, and 15 parts of toluene; the epoxidation rate of the epoxidized natural rubber is 25%, which is provided by the Chinese Academy of Tropical Agricultural Sciences; the hyperbranched polyurethane containing amino groups is made according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN104693405B.

[0043] The thickness of the main rubber layer is 12 mm, the thickness of the surface elastic buffer layer is 1 mm, the thickness of the carbon fiber skeleton modified by the surface elastic buffer layer is 4 mm; and the carbon fiber skeleton is made of carbon fiber cords.

[0044] A method for preparing the carbon fiber reinforced polyurethane rubber synchronous belt comprises the following steps: Step S1, preparation of a carbon fiber skeleton layer modified with a surface elastic buffer layer: after uniformly mixing the raw materials of the surface elastic buffer layer, adding them into a glue machine, uniformly dispersing them by ultrasonic-assisted stirring to obtain glue, then immersing a carbon fiber skeleton made of carbon fiber cords in the glue, taking it out and curing it at 115° C. for 1.5 hours to obtain a carbon fiber skeleton layer modified with a surface elastic buffer layer; Step S2, preparation of the main rubber layer: putting the polyether mixing type polyurethane rubber and the thermoplastic polyester elastomer into an open mill for mixing, alternately adding other raw materials, and mixing evenly to obtain the main rubber layer; Step S3, wrapping and laminating: wrapping and laminating the main adhesive layer and the cloth layer on the carbon fiber skeleton layer modified by the surface elastic buffer layer in the order of the main adhesive layer, the carbon fiber skeleton layer modified by the surface elastic buffer layer and the cloth layer from top to bottom, and then placing it in a synchronous belt mold for pressing and vulcanization, and cooling to room temperature to obtain a carbon fiber reinforced polyurethane rubber synchronous belt; the vulcanization temperature is 180°C, the vulcanization pressure is 10MPa, and the vulcanization time is 35min. Example 4

[0045] A carbon fiber reinforced polyurethane rubber synchronous belt, which comprises, from top to bottom, a main rubber layer, a carbon fiber skeleton layer modified by a surface elastic buffer layer, and a cloth layer; the main rubber layer is made of the following raw materials in parts by weight: 68 parts of polyether mixed polyurethane rubber, 19 parts of thermoplastic polyester elastomer, 1,3-bis(oxiranylmethyl)-5-(2-propylene)-1,3,5-triazine-2,4,6(1H,3H,5 H)-trione 4.5 parts, 3,3'-diamino-4,4'-difluorodiphenyl sulfone 2.5 parts, (3,6-diamino-9-acridinyl)boric acid 2.5 parts, 2-acrylamido-2-methylpropanesulfonic acid 3.5 parts, inorganic filler 23 parts, coupling agent 4.5 parts, vulcanizing agent 3.5 parts, phosphorus pentoxide 2.5 parts, polyphosphoric acid 0.75 parts, antioxidant 2.5 parts, stearic acid 2.5 parts, scorch retarder 0.45 parts.

[0046] The polyether compounded polyurethane rubber is a rubber with an unsaturated structure synthesized by using polyether polyol and 4,4'-diphenylmethane diisocyanate (MDI) as the main raw materials, and its brand is UR101; the thermoplastic polyester elastomer is Riteflex® TPC-ET thermoplastic polyester elastomer; the inorganic filler is a mixture of white carbon black and carbon nanofiber in a mass ratio of 2.5:1; the particle size of the white carbon black is 1400 mesh; the average diameter of the carbon nanofiber is 90nm, and the long diameter is 1.3mm. The ratio is 28:1; the coupling agent is a mixture of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570 in a mass ratio of 1:2:3; the vulcanizing agent is a mixture of tetrapentamethylenethiuram sulfide, vulcanizing agent bis 25, benzoyl peroxide and diisopropylbenzene peroxide in a mass ratio of 1:0.6:0.5:1.1; the antioxidant is a mixture of antioxidant NBC and antioxidant BLE in a mass ratio of 3:5; the anti-scorch agent is anti-scorch agent CTP.

[0047] The surface elastic buffer layer is made of the following raw materials in parts by weight: 65 parts of epoxidized natural rubber, 28 parts of hyperbranched polyurethane containing amino groups, 4.5 parts of trirosin acid glycerol, 2.5 parts of bis(3-aminophenyl)3,5-bis(trifluoromethyl)phenylphosphine oxide, and 18 parts of toluene; the epoxidation rate of the epoxidized natural rubber is 25%, which is provided by the Chinese Academy of Tropical Agricultural Sciences; the hyperbranched polyurethane containing amino groups is made according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN104693405B.

[0048] The thickness of the main rubber layer is 12 mm, the thickness of the surface elastic buffer layer is 1 mm, the thickness of the carbon fiber skeleton modified by the surface elastic buffer layer is 4 mm; and the carbon fiber skeleton is made of carbon fiber cords.

[0049] A method for preparing the carbon fiber reinforced polyurethane rubber synchronous belt comprises the following steps: Step S1, preparation of a carbon fiber skeleton layer modified with a surface elastic buffer layer: after uniformly mixing the raw materials of the surface elastic buffer layer, adding them into a glue machine, uniformly dispersing them by ultrasonic-assisted stirring to obtain glue, then immersing a carbon fiber skeleton made of carbon fiber cords in the glue, taking it out and curing it at 118° C. for 1.8 hours to obtain a carbon fiber skeleton layer modified with a surface elastic buffer layer; Step S2, preparation of the main rubber layer: putting the polyether mixing type polyurethane rubber and the thermoplastic polyester elastomer into an open mill for mixing, alternately adding other raw materials, and mixing evenly to obtain the main rubber layer; Step S3, wrapping and laminating: wrapping and laminating the main adhesive layer and the cloth layer on the carbon fiber skeleton layer modified by the surface elastic buffer layer in the order of the main adhesive layer, the carbon fiber skeleton layer modified by the surface elastic buffer layer and the cloth layer from top to bottom, and then placing it in a synchronous belt mold for pressing and vulcanization, and cooling to room temperature to obtain a carbon fiber reinforced polyurethane rubber synchronous belt; the vulcanization temperature is 185°C, the vulcanization pressure is 11MPa, and the vulcanization time is 38min. Example 5

[0050] A carbon fiber reinforced polyurethane rubber synchronous belt comprises, from top to bottom, a main rubber layer, a carbon fiber skeleton layer modified by a surface elastic buffer layer, and a cloth layer; the main rubber layer is made of the following raw materials in parts by weight: 70 parts of polyether mixed polyurethane rubber, 20 parts of thermoplastic polyester elastomer, 5 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 3 parts of 3,3'-diamino-4,4'-difluorodiphenyl sulfone, 3 parts of (3,6-diamino-9-acridinyl)boric acid, 4 parts of 2-acrylamido-2-methylpropanesulfonic acid, 25 parts of inorganic filler, 5 parts of coupling agent, 4 parts of vulcanizing agent, 3 parts of phosphorus pentoxide, 0.8 parts of polyphosphoric acid, 3 parts of antioxidant, 3 parts of stearic acid, and 0.5 parts of scorch retarder.

[0051] The polyether compounded polyurethane rubber is a rubber with an unsaturated structure synthesized with polyether polyol and 4,4'-diphenylmethane diisocyanate (MDI) as the main raw materials, and its brand is UR101; the thermoplastic polyester elastomer is Riteflex® TPC-ET thermoplastic polyester elastomer; the inorganic filler is a mixture of white carbon black and carbon nanofiber in a mass ratio of 3:1; the particle size of the white carbon black is 1500 mesh; the average diameter of the carbon nanofiber is 100 nm, and the aspect ratio is 30:1.

[0052] The coupling agent is silane coupling agent KH550; the vulcanizing agent is a mixture of dipentamethylenethiuram tetrasulfide, vulcanizing agent bis 25, benzoyl peroxide, and diisopropylbenzene peroxide in a mass ratio of 1:0.7:0.5:1.2; the antioxidant is antioxidant BLE; and the anti-scorch agent is anti-scorch agent CTP.

[0053] The surface elastic buffer layer is made of the following raw materials in parts by weight: 70 parts of epoxidized natural rubber, 30 parts of hyperbranched polyurethane containing amino groups, 5 parts of trirosin acid glycerol, 3 parts of bis(3-aminophenyl)3,5-bis(trifluoromethyl)phenylphosphine oxide, and 20 parts of toluene; the epoxidation rate of the epoxidized natural rubber is 25%, which is provided by the Chinese Academy of Tropical Agricultural Sciences; the hyperbranched polyurethane containing amino groups is made according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN104693405B.

[0054] The thickness of the main rubber layer is 12 mm, the thickness of the surface elastic buffer layer is 1 mm, the thickness of the carbon fiber skeleton modified by the surface elastic buffer layer is 4 mm; and the carbon fiber skeleton is made of carbon fiber cords.

[0055] A method for preparing the carbon fiber reinforced polyurethane rubber synchronous belt comprises the following steps: Step S1, preparation of a carbon fiber skeleton layer modified with a surface elastic buffer layer: after uniformly mixing the raw materials of the surface elastic buffer layer, adding them into a glue machine, uniformly dispersing them by ultrasonic-assisted stirring to obtain glue, then immersing a carbon fiber skeleton made of carbon fiber cords in the glue, taking it out and curing it at 120° C. for 2 hours to obtain a carbon fiber skeleton layer modified with a surface elastic buffer layer; Step S2, preparation of the main rubber layer: putting the polyether mixing type polyurethane rubber and the thermoplastic polyester elastomer into an open mill for mixing, alternately adding other raw materials, and mixing evenly to obtain the main rubber layer; Step S3, wrapping and laminating: wrapping and laminating the main adhesive layer and the cloth layer on the carbon fiber skeleton layer modified by the surface elastic buffer layer in the order of the main adhesive layer, the carbon fiber skeleton layer modified by the surface elastic buffer layer and the cloth layer from top to bottom, and then placing it in a synchronous belt mold for pressing and vulcanization, and cooling to room temperature to obtain a carbon fiber reinforced polyurethane rubber synchronous belt; the vulcanization temperature is 190° C., the vulcanization pressure is 12 MPa, and the vulcanization time is 40 min.

[0056] Comparative Example 1 A carbon fiber reinforced polyurethane rubber synchronous belt and a preparation method thereof, which are substantially the same as those in Example 1, except that 3,3'-diamino-4,4'-difluorodiphenyl sulfone and trirosin acid glycerol are not added.

[0057] Comparative Example 2 A carbon fiber reinforced polyurethane rubber synchronous belt and a preparation method thereof, which are substantially the same as those in Example 1, except that (3,6-diamino-9-acridinyl)boric acid and bis(3-aminophenyl)3,5-bis(trifluoromethyl)phenylphosphine oxide are not added.

[0058] In order to further illustrate the beneficial technical effects of the carbon fiber reinforced polyurethane rubber synchronous belts involved in each embodiment of the present invention, relevant performance tests were carried out on the main rubber layer of the carbon fiber reinforced polyurethane rubber synchronous belts involved in Examples 1-5 and Comparative Examples 1-2 after vulcanization. The test results are shown in Table 1. The test method is as follows: the carbon fiber cords described in each test sample are made of M55J grade high-strength and high-modulus carbon fiber; the aging resistance performance is achieved by placing the main rubber layer of the synchronous belt of each product after vulcanization in hot air at 130°C for artificial accelerated aging for 70 hours, cooling it to room temperature, testing and calculating the main rubber layer of the synchronous belt after vulcanization at room temperature The retention rate of the tensile strength of the rubber layer, the larger the retention rate, the better the heat aging resistance. The tensile strength test of the main rubber layer after vulcanization is carried out in accordance with GB / T528-2009, with a tensile rate of 100mm / min; the low temperature resistance is to place the rubber material of the synchronous belt of each product after vulcanization at -40℃ for 5 hours, and then restore it to room temperature, test and calculate the retention rate of the tensile strength of the main rubber layer of the synchronous belt after vulcanization at room temperature. The larger the retention rate, the better the cold resistance; Akron abrasion is determined according to GB / T1689-1998; the limiting oxygen index of the main rubber layer after vulcanization is carried out according to GB / T 10707-2008.

[0059] As can be seen from Table 1, the carbon fiber reinforced polyurethane rubber synchronous belt disclosed in the embodiment of the present invention has better heat aging resistance, cold resistance and wear resistance than the comparative example product, and has greater strength and better flame retardancy. The addition of 3,3'-diamino-4,4'-difluorodiphenyl sulfone, trirosin acid glycerol, (3,6-diamino-9-acridinyl) boric acid and bis(3-aminophenyl) 3,5-bis(trifluoromethyl)phenylphosphine oxide is beneficial to improving the above properties.

[0060] Table 1

[0061] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.

Claims

1. A carbon fiber reinforced polyurethane rubber synchronous belt, characterized in that: The main rubber layer is made of the following raw materials in parts by weight: 60-70 parts of polyether mixed polyurethane rubber, 10-20 parts of thermoplastic polyester elastomer, 3-5 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione , 1-3 parts of 3,3'-diamino-4,4'-difluorodiphenyl sulfone, 1-3 parts of (3,6-diamino-9-acridinyl)boric acid, 2-4 parts of 2-acrylamido-2-methylpropanesulfonic acid, 15-25 parts of inorganic filler, 3-5 parts of coupling agent, 2-4 parts of vulcanizing agent, 1-3 parts of phosphorus pentoxide, 0.5-0.8 parts of polyphosphoric acid, 1-3 parts of antioxidant, 1-3 parts of stearic acid, and 0.3-0.5 parts of scorch retarder.

2. The carbon fiber reinforced polyurethane rubber synchronous belt according to claim 1, characterized in that: The polyether compounding polyurethane rubber is a rubber with an unsaturated structure synthesized by using polyether polyol and 4,4'-diphenylmethane diisocyanate (MDI) as the main raw materials, and its brand is UR101; the thermoplastic polyester elastomer is Riteflex ® TPC-ET thermoplastic polyester elastomer.

3. The carbon fiber reinforced polyurethane rubber synchronous belt according to claim 1, characterized in that: The inorganic filler is a mixture of white carbon black and carbon nanofibers in a mass ratio of (1-3):1; the particle size of the white carbon black is 1000-1500 mesh; the average diameter of the carbon nanofibers is 50-100nm, and the aspect ratio is (20-30):

1.

4. The carbon fiber reinforced polyurethane rubber synchronous belt according to claim 1, characterized in that: The coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570.

5. The carbon fiber reinforced polyurethane rubber synchronous belt according to claim 1, characterized in that: The vulcanizing agent is a mixture of dipentamethylenethiuram tetrasulfide, vulcanizing agent bis-25, benzoyl peroxide and dicumyl peroxide in a mass ratio of 1:(0.3-0.7):0.5:(0.8-1.2).

6. The carbon fiber reinforced polyurethane rubber synchronous belt according to claim 1, characterized in that: The antioxidant is at least one of antioxidant NBC and antioxidant BLE; the anti-scorching agent is anti-scorching agent CTP.

7. The carbon fiber reinforced polyurethane rubber synchronous belt according to claim 1, characterized in that: The surface elastic buffer layer is made of the following raw materials in parts by weight: 50-70 parts of epoxidized natural rubber, 20-30 parts of amino-containing hyperbranched polyurethane, 3-5 parts of trirosin acid glycerol, 1-3 parts of bis(3-aminophenyl)3,5-bis(trifluoromethyl)phenylphosphine oxide, and 10-20 parts of toluene; the epoxidation rate of the epoxidized natural rubber is 25%.

8. The carbon fiber reinforced polyurethane rubber synchronous belt according to claim 1, characterized in that: The thickness of the main rubber layer is 8-12 mm, the thickness of the surface elastic buffer layer is 1-2 mm, the thickness of the carbon fiber skeleton modified by the surface elastic buffer layer is 4-6 mm; and the carbon fiber skeleton is made of carbon fiber cords.

9. A method for preparing a carbon fiber reinforced polyurethane rubber synchronous belt according to any one of claims 1 to 8, characterized in that: The steps include: Step S1, preparation of a carbon fiber skeleton layer modified with a surface elastic buffer layer: after uniformly mixing the raw materials of the surface elastic buffer layer, adding them into a glue machine, uniformly dispersing them by ultrasonic-assisted stirring to obtain glue, then immersing a carbon fiber skeleton made of carbon fiber cords in the glue, taking it out and curing it at 110-120° C. for 1-2 hours to obtain a carbon fiber skeleton layer modified with a surface elastic buffer layer; Step S2, preparation of the main rubber layer: putting the polyether mixing type polyurethane rubber and the thermoplastic polyester elastomer into an open mill for mixing, alternately adding other raw materials, and mixing evenly to obtain the main rubber layer; Step S3, wrapping and laminating: wrapping and laminating the main adhesive layer and the cloth layer on the carbon fiber skeleton layer modified by the surface elastic buffer layer in the order of main adhesive layer, carbon fiber skeleton layer modified by the surface elastic buffer layer and cloth layer from top to bottom, and then placing it in a synchronous belt mold for pressing and vulcanization, and cooling to room temperature to obtain a carbon fiber reinforced polyurethane rubber synchronous belt.

10. The method for preparing a carbon fiber reinforced polyurethane rubber synchronous belt according to claim 9, characterized in that: In step S3, the vulcanization temperature is 170-190° C., the vulcanization pressure is 8-12 MPa, and the vulcanization time is 30-40 min.

Citation Information

Patent Citations

  • High-temperature-resistant synchronous belt and preparation method thereof

    CN104696437A

  • Synchronous belt and manufacture method thereof

    CN105218909A

  • Tooth-shaped synchronous belt

    CN117489753A

  • Manufacturing method of double-sided tooth synchronous belt

    CN117507442A

  • High-strength carbon fiber synchronous belt and preparation method thereof

    CN118638357A

Cited By

  • Wear-resistant and high-temperature-resistant synchronous belt and preparation method thereof

    CN119552495A

  • Electricity-saving tangential belt for super-long intelligent ring spinning frame and preparation method thereof

    CN119682332A