Carbon black master batch for polyamide 66 civil filament fiber as well as preparation method and application of carbon black master batch

By using nanoscale carbon black powder with a specific particle size and a high-purity dispersant, the problems of equipment clogging and performance degradation caused by the water absorption of polyamide 66 were solved, and the preparation of high-quality carbon black masterbatch and spinning stability were achieved, meeting the requirements of wear resistance and heat resistance of high-quality fibers.

CN118994897APending Publication Date: 2024-11-22FUJIAN EVERSUN JINJIANG CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411093473.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional dyeing processes are energy-intensive and polluting. The water absorption of polyamide 66 leads to equipment blockage and performance degradation. Existing carbon black masterbatches cannot meet the abrasion resistance and heat resistance requirements of high-quality fibers.

Method used

Polyamide 66 carbon black masterbatch is prepared by using nano-sized carbon black powder with specific particle size, fluorinated long-chain alkane amide hydrophobic agent and high-purity single-type carbon black dispersant through a specific process, which improves dispersibility and hydrophobicity, and ensures the stability and high blackness of the spinning process.

Benefits of technology

It achieves efficient and stable carbon black masterbatch production, reduces equipment blockage, improves fiber quality and production continuity, reduces resource consumption, and meets the requirements of green manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994897A_ABST
    Figure CN118994897A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon black master batch for a civil polyamide 66 filament fiber as well as a preparation method and application of the carbon black master batch. Comprising the following components: 56-78% of polyamide 66 slices, 1-3% of a fluoro long-chain alkane amide hydrophobic agent, 20-40% of nanoscale carbon black powder, 1-3% of a single carbon black amide high-purity dispersing agent, 1-3% of an antioxidant, 1-3% of a lubricant and 1-3% of a lubricant. According to the preparation method, the carbon black master batch for the civil polyamide 66 filament fiber is prepared through quantitative feeding, melting plasticizing, screw shearing, water-cooling pelletizing, vibration screening and vacuum drying in sequence, and the carbon black master batch for the civil polyamide 66 filament fiber is directly applied to production of the civil black polyamide 66 filament fiber; the carbon black master batch prepared by the preparation method has high wear resistance, heat resistance and hydrolysis resistance, the produced polyamide 66 black civil filament fiber has few broken ends and high quality, the produced carbon black master batch is suitable for more production processes due to the high melting point, and the problem that polyamide 6 cannot be suitable for various production processes is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of masterbatches, in particular to a carbon black masterbatch for polyamide 66 civilian filament fibers and a preparation method and application thereof. Background Art

[0002] Polyamide is an important class of polymer materials. According to its molecular structure, it can be divided into aliphatic polyamide, aromatic polyamide and semi-aromatic polyamide. Aliphatic polyamide mainly includes two structural types: one is formed by ring-opening polymerization of lactam or condensation of amino acid, such as polyamide 6; the other is formed by condensation of organic dibasic acid and organic diamine, such as polyamide 66. Both polyamide 6 and polyamide 66 are important civilian filament fiber materials. Among them, polyamide 66 occupies an important position in the high-quality fiber market due to its excellent wear resistance, heat resistance and hydrolysis resistance. In contrast, polyamide 6 has a lower melting point, lower crystallinity and rigidity, lower strength and modulus, poorer wear resistance, weaker chemical resistance and hydrolysis resistance, and poorer dimensional stability. These limitations restrict its use in applications that require higher performance. Polyamide 66 occupies an important position in the high-quality fiber market due to its excellent wear resistance, heat resistance and hydrolysis resistance.

[0003] However, the traditional dyeing process not only consumes a lot of energy, but also causes environmental pollution. In order to solve these problems, the industry has begun to turn to more environmentally friendly solution coloring technology. For example, a Chinese patent entitled "A carbon black masterbatch for nylon 6 civilian filament fiber and its preparation method and application" (application number: CN202110490993.5) proposes a carbon black masterbatch preparation scheme based on polyamide 6 chips. Although this method has made some progress in the field of polyamide 6, since the melting point of polyamide 6 is lower than that of polyamide 66, and it is not as good as polyamide 66 in wear resistance, heat resistance and hydrolysis resistance, the carbon black masterbatch produced by it cannot fully meet the needs of high-quality fibers.

[0004] Polyamide 66 itself has strong water absorption because its molecular structure allows water molecules to easily enter the amorphous region and form hydrogen bonds with the amide bonds, resulting in expansion and dimensional changes after water absorption. This water absorption not only affects the fluidity of the material, but may also cause equipment blockage during the production process, interfering with the continuity and stability of production. In addition, excessive water absorption will also reduce the thermal stability of polyamide 66, making it more susceptible to thermal degradation in the molten state, affecting the performance of the final product. Summary of the invention

[0005] The object of the present invention is to provide a carbon black masterbatch for polyamide 66 civilian filament fibers. By using carbon black powder of a specific particle size and a purified and improved single type carbon black high-purity dispersant in the composition, the polyamide 66 carbon black masterbatch has good dispersibility while maintaining high blackness. At the same time, by adding a fluorinated long-chain alkane amide hydrophobic agent, the problem of easy ring clogging of the polyamide 66 masterbatch during the spinning process due to its strong water absorption is improved, thereby further producing civilian polyamide 66 black filament fibers with high blackness and high wear resistance that can be continuously produced.

[0006] To achieve the above object, the present invention is implemented through the following technical solutions:

[0007] A carbon black masterbatch for polyamide 66 civilian filament fiber comprises the following components in weight percentage: 56-78% of polyamide 66 chips, 1-3% of fluorinated long-chain alkane amide hydrophobic agent, 20-40% of nano-scale carbon black powder, and 1-3% of single carbon black amide high-purity dispersant.

[0008] Furthermore, the polyamide 66 slice is a glossy polyamide 66 slice, a semi-dull polyamide 66 slice or a dull polyamide 66 slice.

[0009] Furthermore, the water content of the polyamide 66 chips is 800-1400 ppm, the extractable matter is ≤0.3%, the molecular weight is 24000-34000, and the relative viscosity ranges from 2.45 to 2.70.

[0010] Furthermore, the hydrophobic agent is a fluorinated long-chain alkane amide compound having two alkane chains of equal length, each of which has ≥16 carbon atoms, and the end of the alkane chain contains 0 to 6 CF bonds.

[0011] Furthermore, the nanoscale carbon black powder has a particle size of 25 to 30 nm, an oil absorption value of 70 to 95 mL / 100 g, and a specific surface area of ​​120 to 200 m 2 / g, ash content ≤0.2%, moisture ≤0.8%, tinting strength 110-130%, pH 7-8.

[0012] Furthermore, the single carbon black amide high-purity dispersant is an amide macromolecular compound purified by ethanol hot filtration method, and contains an amide group in its structure.

[0013] Another object of the present invention is to disclose a method for preparing a carbon black masterbatch for polyamide 66 civilian filament fiber, comprising the following steps:

[0014] S1: premixing nano-scale carbon black powder, fluorinated long-chain alkane amide hydrophobic agent and single carbon black high-purity dispersant to obtain a mixture;

[0015] S2: Automatic feeding is adopted to feed the materials, and the polyamide 66 slices are automatically sampled through the main feeding port at a set flow rate; the mixture of step S1 is fed from the side feeding port at a set flow rate, and the two components are successively subjected to melt plasticization, screw transmission and shearing, water-cooled pelletizing, vibration screening and air drying in a parallel co-rotating twin-screw extruder to prepare polyamide 66 civil filament fiber carbon black masterbatch.

[0016] Furthermore, the carbon black masterbatch for polyamide 66 civilian filament fibers obtained after air drying in step S2 has a moisture content of 800 to 1000 ppm and a relative viscosity of 2.19 to 2.35.

[0017] Furthermore, the melt plasticizing process in step S2 is divided into eleven temperature zones and a head temperature zone; the temperature control range of each temperature zone is: 250-270°C in the first temperature zone, 270-290°C in the second temperature zone, 265-285°C in the third temperature zone, 265-285°C in the fourth temperature zone, 250-270°C in the fifth temperature zone, 260-280°C in the sixth temperature zone, 250-270°C in the seventh temperature zone, 235-255°C in the eighth temperature zone, 235-255°C in the ninth temperature zone, 230-250°C in the tenth temperature zone, 230-250°C in the eleventh temperature zone, and 250-290°C in the head temperature zone, wherein the main feeding port is connected to the first temperature zone, and the side feeding port is connected to the fifth temperature zone.

[0018] The invention also discloses a method for preparing carbon black masterbatch for polyamide 66 civilian filament fibers and application of the prepared carbon black masterbatch in polyamide 66 civilian filament fibers.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The present invention adopts polyamide 66 as one of the key components of carbon black masterbatch because of its excellent wear resistance, heat resistance and hydrolysis resistance, which better meets the market demand for high-quality fibers. The carbon black masterbatch based on polyamide 66 chips can better meet the high standards of civil filament fibers for wear resistance, heat resistance and hydrolysis resistance. Due to the high melting point and viscosity characteristics of polyamide 66, the use of suitable raw materials and process parameters can achieve efficient and stable carbon black masterbatch production.

[0021] 2. The present invention proposes to use a fluorinated long-chain alkane amide compound as a high-efficiency hydrophobic agent to improve the production of polyamide 66 carbon black masterbatch. The long-chain alkane in the hydrophobic agent molecule contains a large number of CH2 groups, has low surface tension, can significantly reduce surface energy, and makes it difficult for water molecules to adhere, showing good hydrophobicity. At the same time, the fluoroalkyl group at the end of the molecule is a highly electronegative functional group. The strong polarity of the carbon-fluorine bond causes the electron cloud to be biased towards the fluorine atom, making the fluoroalkyl group show extremely strong hydrophobic properties. In addition, due to the presence of polar amide bonds and non-polar long-chain CH2 structures in its molecular structure, it exhibits a certain lubricity. In the production process of polyamide 66 carbon black masterbatch, this substance can reduce the friction between the masterbatch components and the screw and pipe, reduce wear, and to a certain extent ensure the continuous production of the equipment and extend its service life. More importantly, due to the reduction in friction in the production process, the dust generated in the production process of polyamide 66 carbon black masterbatch is greatly reduced, and the amount of dust adsorbed by the masterbatch itself is also reduced. Excessive dust will block the masterbatch machine sensor during the spinning process of the masterbatch. In severe cases, it will cause frequent machine jumps and affect normal production. Therefore, the hydrophobic agent reduces the dust content of the polyamide 66 carbon black masterbatch through its lubricity, thereby improving the quality of the masterbatch and downstream yarn as well as the continuous production time of spinning. At the same time, the two long chain structures in its molecular structure give it a certain degree of anti-caking properties, which improves the fluidity of polyamide 66 to a certain extent, and avoids the blockage of pipelines or spinning boxes caused by the residual components generated by partial agglomeration of the melt due to too long residence time to form difficult-to-melt gels during the masterbatch production or spinning process. If such blockage occurs in factory production, it is necessary to stop production and cool down, dismantle the pipelines and boxes, and burn and clean them at 800℃. This will seriously affect the continuity of production and bring great economic losses. After adding such hydrophobic agents, the fluidity of the melt is improved to a certain extent, and the occurrence of pipeline and box blockage is greatly reduced, which has high economic benefits. By comparison, the polyamide 66 carbon black masterbatch and the yarn produced after adding such hydrophobic agents have better gloss and color brightness, smoother feel, and improved the market competitiveness of the products.

[0022] 3. The present invention selects nano-scale carbon black powder with a particle size between 25 and 30 nm as one of the key components of carbon black masterbatch. The nano-scale carbon black powder in this particle size range can not only ensure good dispersibility in polyamide 66 chips, but also help improve the dispersibility and fluidity of carbon black masterbatch in the spinning process, reduce equipment blockage, and ensure the stability of fiber quality. It can also prevent ring knots and blockages at the feed port, shorten the cleaning and maintenance time, improve the overall efficiency of the production line, and maintain an excellent blackness value to reduce the use of carbon black, indirectly reducing resource consumption and waste generation, which is in line with the development trend of green manufacturing.

[0023] 4. The single carbon black amide high-purity dispersant used in the present invention is an amide macromolecular compound purified by ethanol hot filtration method, and its molecular weight is in the range of 280 to 780. The long-chain alkyl in the structure makes it have a larger molecular weight and steric hindrance, thereby showing excellent dispersibility. Its structure contains amide groups, which makes its polarity similar to that of polyamide. According to the rule of like dissolves like, it has good miscibility with polyamide 66. Compared with polyether ester dispersants, it has less effect on the viscosity of masterbatch, which can not only effectively improve the dispersibility of carbon black in polyamide 66 melt, but also It improves the heat and weather resistance, flow properties of polyamide fibers, and gives the fibers a certain antistatic effect, reduces yarn breakage during the spinning process, and significantly improves the quality of carbon black masterbatch. This single type of carbon black high-purity dispersant does not need to be compounded in advance with production, ensuring the uniformity of the production quality of carbon black masterbatch and reducing product quality problems caused by fluctuations in dispersant quality. This dispersant can significantly improve the wettability and dispersion stability of nano-scale carbon black in polyamide 66 melt, ensuring that there will be no intermittent breakage during the extrusion drawing process of the extrusion granulator, thereby maintaining production stability.

[0024] 5. Although some manufacturers are currently using polyamide 6 carbon black masterbatch to test the production of polyamide 66 black fiber, because the melting point of polyamide 6 is about 35°C lower than that of polyamide 66, the screw temperature is generally 285-300°C during the spinning process of polyamide 66. At this temperature, polyamide 6 is easily oxidized. In addition, the viscosity of polyamide 6 is relatively low, and the viscosity difference will further affect the dispersion uniformity of carbon black during the blending process with polyamide 66. These differences ultimately lead to a decrease in the strength of the finished black fiber of polyamide 66, an increase in the unevenness of the strips, and it is difficult to achieve industrial application. Therefore, the carbon black masterbatch used for polyamide 66 spinning generally uses polyamide 66 as a carrier, which can avoid the compatibility problem between the carbon black masterbatch and polyamide 66, and ensure that the product properties of polyamide 66 are not affected to the greatest extent. The carbon black masterbatch prepared by the method of the present invention can be directly used in the production of black polyamide 66 civilian filament fibers, with good dyeing effect and continuous and stable spinning production.

[0025] 6. In the preparation process of carbon black masterbatch, the present invention divides the melting and plasticizing zone into eleven temperature zones and a die temperature zone. The main feed port of the equipment is connected to the first temperature zone, and the side feed is set in the fifth temperature zone. Because the dispersant is of high purity and complex structure, it has certain requirements on temperature. If the temperature is too low, the single carbon black high-purity dispersant is not completely melted and cannot play a normal dispersing role in production; if the temperature is too high, part of the structure is decomposed by heat, and it is also unable to play a good dispersing role. The feed port of the single carbon black high-purity dispersant is separated from the feed port of the polyamide 66 slice and set in the middle temperature zone, which can better adjust the temperature of the dispersant feed port and protect it from decomposition due to overheating in the molten state, thereby achieving the best dispersing effect. Therefore, the side feed temperature should be strictly controlled within the range of 250-270°C. The appropriate temperature enables carbon black and polyamide 66 slices to achieve a better blending effect, increase the wettability of carbon black in polyamide 66 slices, and further improve the dispersing effect of carbon black. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the dispersant melting point test chart;

[0027] Figure 2 These are infrared spectra of 4 commercially available amide dispersants;

[0028] Figure 3 This is a comparison chart of the melting points of amide type 2 dispersant before and after purification;

[0029] Figure 4 This is the carbon black masterbatch prepared according to Example 4 of the present invention. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. The described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0031] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources;

[0032] The experimental methods in the following embodiments are conventional methods unless otherwise specified.

[0033] The polyamide 66 chips used in the following examples have a water content of 800-1400 ppm, an extractable matter ≤ 0.3%, a molecular weight of 24000-34000, and a relative viscosity range of 2.45-2.70.

[0034] The nano-scale carbon black powder used in the following examples is in powder form, and the particle size of the nano-scale carbon black powder ranges from 25 to 30 nm, the oil absorption value ranges from 70 to 95 mL / 100 g, and the specific surface area ranges from 120 to 200 m 2 / g, ash content ≤0.2%, moisture ≤0.8%, tinting strength between 110 and 130%, and pH range between 7 and 8.

[0035] In the present invention, the melting point of commercially available amide dispersants and polyether ester dispersants was tested and analyzed. Most of the commercially available long-chain amide dispersants have two melting points, such as Figure 1 As shown in Table 1;

[0036] In the process of melting point testing and analysis of commercially available long-chain amide dispersants, it was found that most long-chain amide dispersants have a double melting point phenomenon. The reason behind this phenomenon is that the process route of traditional dispersant synthesis is outdated, the components do not react fully, and there is an uneven distribution of branches. Impurity components show a low melting point due to short branches. Further, we used infrared spectroscopy technology to conduct an in-depth study of four amide dispersants (labeled as amide 1 to amide 4). The results are as follows: Figure 2 As shown in the figure, amide type 1 dispersant is significantly superior to the other three in purity, so amide type 1 dispersant is the best and is considered to be the best choice. However, due to its high price, amide type 2 dispersant can also achieve the expected effect after purification. In contrast, amide type 3 and amide type 4 have relatively poor dispersion effects due to their insufficient purity.

[0037] Table 1 Melting point of dispersants

[0038]

[0039] Example 1

[0040] The carbon black masterbatch for polyamide 66 civilian filament fiber comprises the following components in percentage by weight: 65.0% of polyamide 66 semi-dull chips, 2% of fluorinated long-chain alkane amide hydrophobic agent, 30.0% of nano-scale carbon black powder and 3.0% of amide 1 dispersant powder.

[0041] The method for preparing carbon black masterbatch for polyamide 66 civilian filament fiber specifically comprises the following steps:

[0042] (1) Mixing: premixing 30.0% of nano-scale carbon black powder with a particle size of 27 nm, 3.0% of amide type 1 dispersant powder, and 2% of fluorinated long-chain alkane amide type hydrophobic agent to obtain a mixture;

[0043] (2) quantitative feeding: 65.0% of fiber-grade polyamide 66 semi-matte chips with a particle size of 2 mm are added to the main feed position of the parallel co-rotating twin-screw extruder granulator through a loss-in-weight scale, and the main feed speed is controlled to be 25 Hz; the mixture obtained in step S1 is added to the side feed position of the parallel co-rotating twin-screw extruder granulator through a loss-in-weight scale, and the side feed speed is controlled to be 25 Hz;

[0044] (3) Melt plasticization: The melt plasticization process is divided into eleven temperature zones and a die temperature zone. The temperature of each temperature zone is controlled as follows: the first zone is 265°C; the second zone is 275°C; the third zone is 275°C; the fourth zone is 275°C; the fifth zone is 270°C; the sixth zone is 265°C; the seventh zone is 260°C; the eighth zone is 255°C; the ninth zone is 250°C; the tenth zone is 245°C; the eleventh zone is 240°C; the die is 275°C;

[0045] (4) Screw transmission and shearing: The main engine speed of screw transmission and shearing is 450r / min;

[0046] (5) Water-cooled pelletizing: The main engine speed of the pelletizer for water-cooled pelletizing is 450r / min;

[0047] (6) Vibration screening: The mesh diameter of the vibration screening is 3 mm;

[0048] (7) Blast drying: A carbon black masterbatch for polyamide 66 civilian filament fiber with a moisture content of 800 ppm and a relative viscosity of 2.27 was prepared.

[0049] Example 2

[0050] The carbon black masterbatch for polyamide 66 civilian filament fiber comprises the following components in percentage by weight: 78% of polyamide 66 light slices, 1% of fluorinated long-chain alkane amide hydrophobic agent, 20.0% of nano-scale carbon black powder and 1% of amide type 1 dispersant.

[0051] The method for preparing carbon black masterbatch for polyamide 66 civilian filament fiber specifically comprises the following steps:

[0052] (1) Mixing: 20.0% of nano-scale carbon black powder with a particle size of 25 nm, 1.0% of an amide type 1 dispersant, and 1% of a fluorinated long-chain alkane amide type hydrophobic agent are premixed to obtain a mixture;

[0053] (2) quantitative feeding: 78% of fiber-grade polyamide 66 glossy chips with a particle size of 3 mm are added to the main feeding position of the parallel co-rotating twin-screw extruder granulator through a loss-in-weight scale, and the feeding speed of the main feeding position is controlled to be 23 Hz; the mixture obtained in step S1 is added to the side feeding position of the parallel co-rotating twin-screw extruder granulator through a loss-in-weight scale, and the feeding speed of the side feeding position is controlled to be 27 Hz;

[0054] (3) Melt plasticization: The melt plasticization process is divided into eleven temperature zones and a die temperature zone. The temperature of each temperature zone is controlled as follows: the first zone is 250°C; the second zone is 270°C; the third zone is 265°C; the fourth zone is 265°C; the fifth zone is 250°C; the sixth zone is 260°C; the seventh zone is 250°C; the eighth zone is 235°C; the ninth zone is 235°C; the tenth zone is 230°C; the eleventh zone is 230°C; the die is 250°C;

[0055] (4) Screw transmission and shearing: The main engine speed of screw transmission and shearing is 650r / min;

[0056] (5) Water-cooled pelletizing: The main engine speed of the pelletizer for water-cooled pelletizing is 400r / min;

[0057] (6) Vibration screening: The mesh diameter of the vibration screening is 3 mm;

[0058] (7) Blast drying: A carbon black masterbatch for polyamide 66 civilian filament fiber with a moisture content of 1000 ppm and a relative viscosity of 2.35 was prepared.

[0059] Example 3

[0060] The carbon black masterbatch for polyamide 66 civilian filament fiber comprises the following components in percentage by weight: 56.0% of polyamide 66 matte chips, 2% of fluorinated long-chain alkane amide hydrophobic agent, 40.0% of nano-scale carbon black powder and 2.0% of amide 1 dispersant powder.

[0061] The method for preparing carbon black masterbatch for polyamide 66 civilian filament fiber specifically comprises the following steps:

[0062] (1) Mixing: 40.0% of nano-scale carbon black powder with a particle size of 30 nm, 2.0% of amide type 2 dispersant powder, and 3% of fluorinated long-chain alkane amide type hydrophobic agent are pre-mixed to obtain a mixture;

[0063] (2) quantitative feeding: 56.0% of fiber-grade polyamide 66 matte chips with a particle size of 2 mm are added to the main feed position of the parallel co-rotating twin-screw extruder granulator through a loss-in-weight scale, and the main feed speed is controlled to be 25 Hz; the mixture obtained in step S1 is added to the side feed position of the parallel co-rotating twin-screw extruder granulator through a loss-in-weight scale, and the side feed speed is controlled to be 25 Hz;

[0064] (3) Melt plasticization: The melt plasticization process is divided into eleven temperature zones and a die temperature zone. The temperature of each temperature zone is controlled as follows: the first zone is 270°C; the second zone is 290°C; the third zone is 285°C; the fourth zone is 285°C; the fifth zone is 260°C; the sixth zone is 280°C; the seventh zone is 270°C; the eighth zone is 245°C; the ninth zone is 255°C; the tenth zone is 250°C; the eleventh zone is 250°C; the die is 290°C;

[0065] (4) Screw transmission and shearing: The main engine speed of screw transmission and shearing is 450r / min;

[0066] (5) Water-cooled pelletizing: The main engine speed of the pelletizer for water-cooled pelletizing is 450r / min;

[0067] (6) Vibration screening: The mesh diameter of the vibration screening is 3 mm;

[0068] (7) Blast drying: A carbon black masterbatch for polyamide 66 civilian filament fiber with a moisture content of 900 ppm and a relative viscosity of 2.19 was prepared.

[0069] Example 4

[0070] Except that the dispersant was replaced with amide 2, other process conditions were the same as those in Example 1;

[0071] Example 5

[0072] Except that the dispersant was replaced with amide 2 purified by hot filtration of ethanol, other process conditions were the same as those in Example 1.

[0073] The specific operation of purifying the amide type 2 dispersant includes the following steps: first, dissolving 500g of the amide type 2 dispersant in 1L of anhydrous ethanol; then, heating at 60°C for 30min to promote the dissolution and separation of impurities; then, filtering while hot using a vacuum filtration device to collect the resulting filter residue; finally, removing the residual solvent through a vacuum drying process to obtain a high-purity dispersant. Figure 3 The purified amide type 2 dispersant not only has a significantly decreased low melting point peak, but also has a significantly improved dispersion effect.

[0074] Comparative Example 1

[0075] Except that the die temperature is set to 320° C. during the melt plasticization process in step (3), other processes are the same as in Example 1.

[0076] In the preparation process of carbon black masterbatch, due to the excessively high temperature setting of the screw temperature zone, high-frequency intermittent strand breakage will occur during the extrusion process, causing production abnormalities and making it impossible to stably produce carbon black masterbatch.

[0077] Comparative Example 2

[0078] Except that no dispersant was added, other process conditions were the same as those in Example 1.

[0079] In the preparation process of carbon black masterbatch, due to the lack of dispersant, carbon black agglomerates, resulting in high-frequency intermittent strand breakage during the extrusion process, causing production abnormalities and making it impossible to stably produce carbon black masterbatch.

[0080] Comparative Example 3

[0081] Except that the main feed is changed from 65.0% of fiber-grade polyamide 66 semi-bright chips with a particle size of 2 mm to 67.0% of fiber-grade polyamide 66 semi-matt chips with a particle size of 2 mm, and 2% of fluorinated long-chain alkane amide hydrophobic agent is not added to the side feed, other process conditions are the same as those in Example 1.

[0082] Comparative Example 4

[0083] Except that the dispersant was replaced with amide 3, other process conditions were the same as those in Example 1;

[0084] Comparative Example 5

[0085] Except that the dispersant was replaced with amide 4, other process conditions were the same as those in Example 1;

[0086] Comparative Example 6

[0087] Except that the dispersant was replaced with polyetherester 1, other process conditions were the same as those in Example 1;

[0088] Comparative Example 7

[0089] Except that the dispersant was replaced with polyetherester 2, other process conditions were the same as those in Example 1;

[0090] Performance Testing

[0091] 1. Figure 4 This is a physical picture of the carbon black masterbatch prepared according to the method provided by the present invention. The carbon black masterbatch for polyamide 66 civilian filament fiber is in granular form.

[0092] 2. The physical property test results of the carbon black masterbatch for polyamide 66 civilian filament fiber prepared according to Examples 1 to 5 and Comparative Examples 1 to 7 are shown in Table 2.

[0093] Table 2 Physical properties of polyamide 66 carbon black masterbatch

[0094]

[0095] Note: Since the masterbatch could not be obtained in Comparative Examples 1 and 2, it is not listed

[0096] 3. The application of the carbon black masterbatch for polyamide 66 civilian filament fiber prepared in the above Examples 1 to 5 and Comparative Examples 1 to 7 in downstream spinning is shown in Table 3.

[0097] Table 3 Spinning of polyamide 66 carbon black masterbatch for 40D / 34F FDY fiber

[0098]

[0099] Note: Since the masterbatch could not be obtained in Comparative Examples 1 and 2, it is not listed

[0100] From the test data in Table 2 and Table 3, it can be seen that although the polyether ester hyperdispersants widely used in the market can avoid the problem of component differences caused by frequent compounding, due to the large molecular weight of this type of dispersant, it will reduce the viscosity of the masterbatch to a certain extent, resulting in more floating and broken ends in the subsequent spinning process, and the fiber breaking strength will also decrease, which does not meet the high strength requirements of polyamide 66. In contrast, amide dispersants have less effect on the viscosity of the masterbatch, but their purity is difficult to control. Most of these dispersants on the market contain more short-chain impurities, which will reduce their dispersion effect and also increase the frequency of floating and broken ends in the spinning process.

[0101] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A carbon black masterbatch for polyamide 66 civilian filament fiber, characterized in that: The invention comprises the following components in weight percentage: 56-78% of polyamide 66 slices, 1-3% of fluorinated long-chain alkane amide hydrophobic agent, 20-40% of nanometer-grade carbon black powder and 1-3% of single carbon black amide high-purity dispersant.

2. The carbon black masterbatch for polyamide 66 civilian filament fiber according to claim 1, characterized in that: The polyamide 66 slices are glossy polyamide 66 slices, semi-dull polyamide 66 slices or dull polyamide 66 slices.

3. The carbon black masterbatch for polyamide 66 civilian filament fiber according to claim 2, characterized in that: The water content of polyamide 66 chips is 800-1400 ppm, the extractable matter is ≤0.3%, the molecular weight is 24000-34000, and the relative viscosity ranges from 2.45 to 2.

70.

4. The carbon black masterbatch for polyamide 66 civilian filament fiber according to claim 1, characterized in that: The fluorinated long-chain alkane amide hydrophobic agent has two alkane chains, the two alkane chains are of equal length, and the number of carbon atoms in each alkane chain is ≥16, and the end of the alkane chain contains 0 to 6 CF bonds.

5. The carbon black masterbatch for polyamide 66 civilian filament fiber according to claim 1, characterized in that: The particle size of nano-scale carbon black powder is 25-30nm, the oil absorption value is 70-95mL / 100g, and the specific surface area is 120-200m 2 / g, ash content ≤0.2%, moisture ≤0.8%, tinting strength 110-130%, pH 7-8.

6. The carbon black masterbatch for polyamide 66 civilian filament fiber according to claim 1, characterized in that: The single carbon black amide high-purity dispersant is an amide macromolecular compound purified by ethanol hot filtration method, and contains amide groups in its structure.

7. A method for preparing carbon black masterbatch for polyamide 66 civilian filament fiber as claimed in claim 1, characterized in that: The following steps are involved: S1: premixing nano-scale carbon black powder, fluorinated long-chain alkane amide hydrophobic agent and single carbon black high-purity dispersant to obtain a mixture; S2: Automatic feeding is adopted to feed the materials, and the polyamide 66 slices are automatically sampled through the main feeding port at a set flow rate; the mixture of step S1 is fed from the side feeding port at a set flow rate, and the two components are successively subjected to melt plasticization, screw transmission and shearing, water-cooled pelletizing, vibration screening and air drying in a parallel co-rotating twin-screw extruder to prepare polyamide 66 civil filament fiber carbon black masterbatch.

8. The preparation method according to claim 7, characterized in that: The carbon black masterbatch for polyamide 66 civilian filament fiber obtained after air drying in step S2 has a moisture content of 800 to 1000 ppm and a relative viscosity of 2.19 to 2.

35.

9. The preparation method according to claim 7, characterized in that: In step S2, the melt plasticization process is divided into eleven temperature zones and a die temperature zone; the temperature control range of each temperature zone is: 250-270°C in the first temperature zone, 270-290°C in the second temperature zone, 265-285°C in the third temperature zone, 265-285°C in the fourth temperature zone, 250-270°C in the fifth temperature zone, 260-280°C in the sixth temperature zone, 250-270°C in the seventh temperature zone, 235-255°C in the eighth temperature zone, 235-255°C in the ninth temperature zone, 230-250°C in the tenth temperature zone, 230-250°C in the eleventh temperature zone, and 250-290°C in the die temperature zone, wherein the main feeding port is connected to the first temperature zone, and the side feeding port is connected to the fifth temperature zone.

10. Use of the carbon black masterbatch for polyamide 66 civil filament fibers as claimed in any one of claims 1 to 6 in polyamide 66 civil filament fibers.

Citation Information

Patent Citations

  • High-color carbon black-polyamide color master batch and preparation method thereof

    CN112745674A

  • Carbon black master batch for chinlon 6 civil filament fiber as well as preparation method and application of carbon black master batch

    CN113321929A

  • Polyamide color master batch colored by high-content carbon black for spinning and preparation method of polyamide color master batch

    CN114605769A

  • Carbon black master batch, preparation method thereof and preparation method of superfine denier black chinlon 6

    CN116731506A

  • Compounds made of polyamide substance(s) and perfluoroalkyl substance(s) and mixtures of these compounds with additional polymer substance(s), methods for their production and use

    US6770378B1