Bamboo charcoal modified polypyrrole composite material and preparation method thereof

The preparation of bamboo charcoal/polypyrrole composite materials through electrochemical polymerization has solved the limitations of polypyrrole materials in terms of mechanical stability and cycle life, achieved efficient and environmentally friendly electrochemical performance improvement, and solved the environmental pollution of traditional chemical synthesis methods question.

CN118994902APending Publication Date: 2024-11-22XI'AN POLYTECHNIC UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410999364.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Pure polypyrrole materials have limitations in mechanical stability and cycle life, which limits their wide application in commercial applications, and the existing chemical synthesis methods are cumbersome and have serious environmental pollution.

Method used

The bamboo charcoal/polypyrrole composite material is prepared by electrochemical polymerization method. By initiating a pyrrole polymerization reaction on the electrode surface, the porosity and high specific surface area of ​​the bamboo charcoal are combined to improve the energy storage and environmental friendliness of the material. Specific steps include the preparation of the base electrode, the preparation of the electrolyte and the preparation of the working electrode, the electrochemical polymerization using cyclic voltammetry, and the optimization of the bamboo charcoal dispersion solution concentration and electrolyte composition.

Benefits of technology

The preparation of environmentally friendly and green bamboo charcoal modified polypyrrole composite material has been realized, which improves the specific capacitance and electrochemical performance of the material, significantly improves the energy storage and stability of polypyrrole, and avoids the environmental pollution problem of traditional chemical synthesis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994902A_ABST
    Figure CN118994902A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a bamboo charcoal modified polypyrrole composite material. The preparation method comprises the following steps: firstly, preparing a matrix electrode; then preparing an electrolyte; and finally preparing a working electrode. The invention further discloses the bamboo charcoal modified polypyrrole composite material. The problems that in the prior art, a polypyrrole chemical synthesis method is tedious, and environmental pollution is serious are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and in particular relates to a bamboo charcoal modified polypyrrole composite material. The invention also relates to a preparation method of the bamboo charcoal modified polypyrrole composite material. Background Art

[0002] Bamboo charcoal can not only purify the air, eliminate odors, absorb moisture and prevent mildew, but also inhibit bacteria and repel insects. When in contact with the human body, it helps to remove moisture and absorb sweat, promote blood circulation and metabolism, and relieve fatigue. After scientific refining and processing, bamboo charcoal has been widely used in daily life.

[0003] Polypyrrole has broad application prospects in energy storage technologies such as supercapacitors and lithium-ion batteries, showing great potential. However, the limitations of pure polypyrrole materials in mechanical stability and cycle life restrict its widespread use in commercial applications. To overcome these challenges, researchers are working on developing composite materials of polypyrrole and carbon materials to improve their comprehensive performance.

[0004] Bamboo charcoal, as a natural and renewable carbon resource, has become a preferred material for improving the insufficient energy storage of polypyrrole due to its high specific surface area, excellent chemical stability and environmental friendliness. The porosity of bamboo charcoal can provide polypyrrole with abundant active sites and enhanced electrolyte permeability, which can alleviate the volume expansion of polypyrrole during the charge and discharge process and improve the energy storage of polypyrrole composite materials.

[0005] The bamboo charcoal / polypyrrole composite material was prepared by electrochemical polymerization. This method initiates the polymerization reaction of pyrrole on the electrode surface to prepare the bamboo charcoal / polypyrrole composite material with excellent energy storage properties. Summary of the invention

[0006] The purpose of the present invention is to provide a clean preparation method of a bamboo charcoal modified polypyrrole composite material, which solves the problems of complicated chemical synthesis methods of polypyrrole and serious environmental pollution.

[0007] Another object of the present invention is to provide a bamboo charcoal modified polypyrrole composite material.

[0008] The first technical solution adopted by the present invention is a method for preparing a bamboo charcoal modified polypyrrole composite material, which is specifically implemented according to the following steps:

[0009] Step 1, preparation of substrate electrode;

[0010] Step 2, preparation of electrolyte;

[0011] Step 3: Preparation of working electrode.

[0012] The first technical solution of the present invention is also characterized in that:

[0013] Step 1 is implemented as follows:

[0014] Step 1.1, take out the lead of a 2B pencil and cut it into small pieces of 1-2 cm, use sandpaper to smooth both sides of the small piece of pencil lead and ensure that the effective length is the required length;

[0015] Step 1.2, the small pencil lead after step 1.1 is ultrasonically cleaned in nitric acid aqueous solution and distilled water for 5-15 minutes respectively to remove impurities, taken out and dried for later use;

[0016] Step 1.3, polish the surface of the pencil lead that has been dried in step 1.2, cut a length of enameled copper wire, remove the enameled film on the surface of the copper wire by soaking it in sulfuric acid, and process it until the copper wire is exposed at both ends to make it conductive, then wrap one end of the copper wire around one side of the polished pencil lead and fix it with a 1:1 mixture of AB glue.

[0017] In step 1.2, the volume ratio of nitric acid to water in the nitric acid aqueous solution is 1:1 to 1:2; and the ultrasonic cleaning time is 5 to 15 minutes.

[0018] The intercepted length in step 1.3 is 1.0-2.0 cm.

[0019] Step 2 is implemented as follows:

[0020] Prepare 250-1000 ml of 0.1-1.0 mol / L sulfuric acid solution, 250-500 ml of 0.1-0.3 mol / L pyrrole solution, and 250-500 ml of 0.05-0.6 mol / L potassium sulfate solution respectively.

[0021] Step 3 is implemented as follows:

[0022] Step 3.1, preparation of polypyrrole electrode: select a pencil lead with a length of 1-2 cm as the electrode substrate, ensure that its surface is clean and free of impurities, immerse the pencil lead electrode in an electrolyte, perform electrochemical polymerization using cyclic voltammetry CV, and scrape off the surface of the pencil lead after drying to obtain polypyrrole;

[0023] Step 3.2, preparation of bamboo charcoal / polypyrrole electrode: Soak the pencil core electrode in bamboo charcoal dispersion solution for 5-20 minutes to obtain a bamboo charcoal / pencil core electrode, place it in an electrolyte with pyrrole concentration, K2SO4 concentration, and H2SO4 concentration, and use cyclic voltammetry CV to perform electrochemical polymerization. After drying, scrape it from the surface of the pencil core to obtain bamboo charcoal / polypyrrole.

[0024] The electrolyte in step 3.1 has a pyrrole concentration of 0.1-0.3 mol / L, a K2SO4 concentration of 0.05-0.6 mol / L, and a H2SO4 concentration of 0.1-1 mol / L.

[0025] When cyclic voltammetry (CV) is used for electrochemical polymerization in step 3.1, the scan rate is set to 0.01-0.5 V / s, and 4-16 cycles are scanned in the potential range of -0.1 V to 0.6 V, 0 V to 0.6 V, and -0.2 to 0.6 V.

[0026] The concentration of the bamboo charcoal dispersion solution in step 3.2 is 1-9 mg / ml, and the soaking time is 5-20 min.

[0027] The second technical solution adopted by the present invention is a bamboo charcoal modified polypyrrole composite material prepared by a preparation method of a bamboo charcoal modified polypyrrole composite material.

[0028] The beneficial effect of the present invention is that the preparation method of the bamboo charcoal modified polypyrrole composite material, the environmentally friendly green bamboo charcoal with strong adsorption improves the specific capacitance of polypyrrole, which is the advantage and positive effect of the material of the present invention compared with the existing materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a diagram for optimizing bamboo charcoal concentration in the method for preparing the bamboo charcoal-modified polypyrrole composite material of the present invention;

[0030] Figure 2 It is a cyclic voltammetry curve of bamboo charcoal / polypyrrole in the preparation method of the bamboo charcoal modified polypyrrole composite material of the present invention;

[0031] Figure 3 This is a diagram of an experimental device for a three-electrode working system in the method for preparing a bamboo charcoal-modified polypyrrole composite material of the present invention;

[0032] FIG4( a ) is a multi-scan image of pyrrole on the surface of PEC in the preparation method of the bamboo charcoal modified polypyrrole composite material of the present invention;

[0033] FIG4( b ) is a multi-scan image of pyrrole on the bamboo charcoal / PEC surface in the preparation method of the bamboo charcoal modified polypyrrole composite material of the present invention;

[0034] FIG5( a ) is a diagram showing the drying of a sample prepared in the method for preparing a bamboo charcoal-modified polypyrrole composite material of the present invention;

[0035] FIG5( b ) is a bamboo charcoal / polypyrrole composite material scraped off the bamboo charcoal / pencil lead in the preparation method of the bamboo charcoal modified polypyrrole composite material of the present invention;

[0036] Figure 6 It is a material charge and discharge curve diagram in the preparation method of the bamboo charcoal modified polypyrrole composite material of the present invention. DETAILED DESCRIPTION

[0037] The present invention is described in detail with reference to the accompanying drawings and specific embodiments.

[0038] The preparation method of the bamboo charcoal modified polypyrrole composite material of the present invention is specifically implemented according to the following steps:

[0039] Step 1, preparation of substrate electrode;

[0040] Step 1 is implemented as follows:

[0041] Step 1.1, take out the lead of a 2B pencil and cut it into small pieces of 1-2.0 cm, use sandpaper to smooth both sides of the small piece of pencil lead and ensure that the effective length is the required length;

[0042] Step 1.2, the small pencil lead after step 1.1 is ultrasonically cleaned in nitric acid aqueous solution and distilled water for 5-10 minutes respectively to remove impurities, taken out and dried for later use;

[0043] Step 1.3, polish the surface of the pencil lead that has been dried in step 1.2, cut a length of enameled copper wire, remove the enameled film on the surface of the copper wire by soaking it in sulfuric acid, and process it until the copper wire is exposed at both ends to make it conductive, then wrap one end of the copper wire around one side of the polished pencil lead and fix it with a 1:1 mixture of AB glue.

[0044] In step 1.2, the volume ratio of nitric acid to water in the nitric acid aqueous solution is 1:1 to 1:2; and the ultrasonic cleaning time is 5 to 10 minutes.

[0045] The cut length in step 1.3 is 1-2 cm.

[0046] Step 2, preparation of electrolyte;

[0047] Step 2 is implemented as follows:

[0048] Prepare 250-1000 ml of 0.1-1.0 mol / L sulfuric acid solution: measure 1.34-53.5 ml of sulfuric acid, add enough distilled water, dilute and make up to 250-1000 ml in a volumetric flask;

[0049] Prepare 100-500 ml of 0.1-0.3 mol / L pyrrole solution: weigh 0.6709-10.06 g pyrrole, add distilled water to dissolve, and then dilute to 250-500 ml volumetric flask.

[0050] Prepare 100-500 ml of 0.05-0.6 mol / L potassium sulfate solution: weigh 0.8713-52.28 g potassium sulfate, dissolve it in deionized water, and dilute to 100-500 ml in a volumetric flask.

[0051] Step 3: Preparation of working electrode.

[0052] Step 3 is implemented as follows:

[0053] Step 3.1, preparation of polypyrrole electrode: select a pencil lead with a length of 1-2 cm as the electrode substrate, ensure that its surface is clean and free of impurities, immerse the pencil lead electrode in an electrolyte (pyrrole concentration is 0.1-0.3 mol / L, K2SO4 concentration is 0.05-0.6 mol / L, H2SO4 concentration is 0.1-1 mol / L), use cyclic voltammetry CV to perform electrochemical polymerization, and scrape off the surface of the pencil lead after drying to obtain polypyrrole;

[0054] Step 3.2, preparation of bamboo charcoal / polypyrrole electrode: Soak the pencil core electrode in bamboo charcoal dispersion solution for 5-20 minutes to obtain a bamboo charcoal / pencil core electrode, place it in an electrolyte with a pyrrole concentration of 0.1-0.3 mol / L, a K2SO4 concentration of 0.05-0.6 mol / L, and a H2SO4 concentration of 0.1-1 mol / L, and perform electrochemical polymerization using cyclic voltammetry CV. After drying, scrape it from the surface of the pencil core to obtain bamboo charcoal / polypyrrole.

[0055] The electrolyte in step 3.1 has a pyrrole concentration of 0.1-0.3 mol / L, a K2SO4 concentration of 0.05-0.6 mol / L, and a H2SO4 concentration of 0.1-1 mol / L;

[0056] When cyclic voltammetry (CV) is used for electrochemical polymerization in step 3.1, the scan rate is set to 0.01-0.5 V / s, and 4-16 cycles are scanned in the potential range of -0.1 V to 0.6 V, 0 V to 0.6 V, and -0.2 to 0.6 V.

[0057] The concentration of the bamboo charcoal dispersion solution in step 3.2 is 1-9 mg / ml, and the soaking time is 5-20 min.

[0058] The invention discloses a bamboo charcoal modified polypyrrole composite material prepared by a method for preparing a bamboo charcoal modified polypyrrole composite material.

[0059] Example 1

[0060] The preparation method of the bamboo charcoal modified polypyrrole composite material of the present invention is specifically implemented according to the following steps:

[0061] Step 1, preparation of substrate electrode;

[0062] Step 2, preparation of electrolyte;

[0063] Step 3: Preparation of working electrode.

[0064] Example 2

[0065] The preparation method of the bamboo charcoal modified polypyrrole composite material of the present invention is specifically implemented according to the following steps:

[0066] Step 1, preparation of substrate electrode;

[0067] Step 1 is implemented as follows:

[0068] Step 1.1, take out the lead of a 2B pencil and cut it into 1 cm small pieces of pencil lead, use sandpaper to smooth both sides of the small piece of pencil lead and ensure that the effective length is the required length;

[0069] Step 1.2, the small pencil lead after step 1.1 is ultrasonically cleaned in nitric acid aqueous solution and distilled water for 5 minutes respectively to remove impurities, taken out and dried for later use;

[0070] Step 1.3, polish the surface of the pencil lead that has been dried in step 1.2, cut a length of enameled copper wire, remove the enameled film on the surface of the copper wire by soaking it in sulfuric acid, and process it until the copper wire is exposed at both ends to make it conductive, then wrap one end of the copper wire around one side of the polished pencil lead and fix it with a 1:1 mixture of AB glue.

[0071] In step 1.2, the volume ratio of nitric acid to water in the nitric acid aqueous solution is 1:1; and the ultrasonic cleaning time is 5 minutes.

[0072] The cut length in step 1.3 is 1 cm.

[0073] Step 2, preparation of electrolyte;

[0074] Step 2 is implemented as follows:

[0075] Prepare 250 ml of 0.1 mol / L sulfuric acid solution: measure 1.34 ml of sulfuric acid, add enough distilled water, dilute and make up to 250 ml in a volumetric flask;

[0076] Prepare 100 ml of 0.1 mol / L pyrrole solution: weigh 0.6709 g of pyrrole, add distilled water to dissolve, and then dilute to 100 ml.

[0077] Prepare 100 ml of 0.05 mol / L potassium sulfate solution: weigh 0.8713 potassium sulfate, dissolve it in deionized water, and dilute to 100 ml in a volumetric flask.

[0078] Step 3: Preparation of working electrode.

[0079] Step 3 is implemented as follows:

[0080] Step 3.1, preparation of polypyrrole electrode: select a pencil lead with a length of 1 cm as the electrode substrate, ensure that its surface is clean and free of impurities, immerse the pencil lead electrode in the electrolyte, perform electrochemical polymerization using cyclic voltammetry CV, and scrape off the surface of the pencil lead after drying to obtain polypyrrole;

[0081] Step 3.2, preparation of bamboo charcoal / polypyrrole electrode: Soak the pencil core electrode in bamboo charcoal dispersion solution for 5 minutes to obtain a bamboo charcoal / pencil core electrode, place it in an electrolyte with a pyrrole concentration of 0.1 mol / L, a K2SO4 concentration of 0.05 mol / L, and a H2SO4 concentration of 0.1 mol / L, and perform electrochemical polymerization using cyclic voltammetry CV. After drying, scrape it from the surface of the pencil core to obtain bamboo charcoal / polypyrrole.

[0082] The electrolyte in step 3.1 has a pyrrole concentration of 0.1 mol / L, a K2SO4 concentration of 0.05 mol / L, and a H2SO4 concentration of 0.1 mol / L;

[0083] When cyclic voltammetry (CV) is used for electrochemical polymerization in step 3.1, the scan rate is set to 0.01 V / s, and 4 cycles are scanned in the potential range of -0.1 V to 0.6 V.

[0084] The concentration of the bamboo charcoal dispersion solution in step 3.2 is 1 mg / ml, and the immersion time is 5 min.

[0085] Example 3

[0086] The preparation method of the bamboo charcoal modified polypyrrole composite material of the present invention is specifically implemented according to the following steps:

[0087] Step 1, preparation of substrate electrode;

[0088] Step 1 is implemented as follows:

[0089] Step 1.1, take out the lead of a 2B pencil and cut it into a small piece of pencil lead of 2.0 cm, use sandpaper to smooth both sides of the small piece of pencil lead and ensure that the effective length is the required length;

[0090] Step 1.2, the small pencil lead after step 1.1 is ultrasonically cleaned in nitric acid aqueous solution and distilled water for 10 minutes respectively to remove impurities, taken out and dried for later use;

[0091] Step 1.3, polish the surface of the pencil lead that has been dried in step 1.2, cut a length of enameled copper wire, remove the enameled film on the surface of the copper wire by soaking it in sulfuric acid, and process it until the copper wire is exposed at both ends to make it conductive, then wrap one end of the copper wire around one side of the polished pencil lead and fix it with a 1:1 mixture of AB glue.

[0092] In step 1.2, the volume ratio of nitric acid to water in the nitric acid aqueous solution is 1:2; and the ultrasonic cleaning time is 10 minutes.

[0093] The cut length in step 1.3 is 2 cm.

[0094] Step 2, preparation of electrolyte;

[0095] Step 2 is implemented as follows:

[0096] Prepare 1000 ml of 1 mol / L sulfuric acid solution: measure 53.5 ml of sulfuric acid, add enough distilled water, dilute and make up to 1000 ml in a volumetric flask;

[0097] Prepare 500 ml of 0.3 mol / L pyrrole solution: weigh 10.06 g of pyrrole, add distilled water to dissolve, and then dilute to 500 ml in a volumetric flask.

[0098] Prepare 500 ml of 0.6 mol / L potassium sulfate solution: weigh 52.28 g of potassium sulfate, dissolve it in deionized water, and dilute to 500 ml in a volumetric flask.

[0099] Step 3: Preparation of working electrode.

[0100] Step 3 is implemented as follows:

[0101] Step 3.1, preparation of polypyrrole electrode: select a pencil lead with a length of 2 cm as the electrode substrate, ensure that its surface is clean and free of impurities, immerse the pencil lead electrode in an electrolyte (pyrrole concentration is 0.3 mol / L, K2SO4 concentration is 0.6 mol / L, H2SO4 concentration is 1 mol / L), and use cyclic voltammetry CV to perform electrochemical polymerization. After drying, scrape off the surface of the pencil lead to obtain polypyrrole;

[0102] Step 3.2, preparation of bamboo charcoal / polypyrrole electrode: Soak the pencil core electrode in the bamboo charcoal dispersion solution for 20 minutes to obtain the bamboo charcoal / pencil core electrode, place it in the electrolyte, and use cyclic voltammetry CV to perform electrochemical polymerization. After drying, scrape it from the surface of the pencil core to obtain bamboo charcoal / polypyrrole.

[0103] The electrolyte in step 3.1 has a pyrrole concentration of 0.3 mol / L, a K2SO4 concentration of 0.6 mol / L, and a H2SO4 concentration of 1 mol / L;

[0104] When cyclic voltammetry (CV) is used for electrochemical polymerization in step 3.1, the scan rate is set to 0.5 V / s, and 16 cycles are scanned in the potential range of 0 V to 0.6 V.

[0105] The concentration of the bamboo charcoal dispersion solution in step 3.2 is 9 mg / ml, and the immersion time is 20 min.

[0106] Example 4

[0107] The preparation method of the bamboo charcoal modified polypyrrole composite material of the present invention is specifically implemented according to the following steps:

[0108] Step 1, preparation of substrate electrode;

[0109] Step 1 is implemented as follows:

[0110] Step 1.1, take out the lead of a 2B pencil and cut it into 1.5 cm small pieces of pencil lead, use sandpaper to smooth both sides of the small piece of pencil lead and ensure that the effective length is the required length;

[0111] Step 1.2, the small pencil lead after step 1.1 is ultrasonically cleaned in nitric acid aqueous solution and distilled water for 8 minutes respectively to remove impurities, taken out and dried for later use;

[0112] Step 1.3, polish the surface of the pencil lead that has been dried in step 1.2, cut a length of enameled copper wire, remove the enameled film on the surface of the copper wire by soaking it in sulfuric acid, and process it until the copper wire is exposed at both ends to make it conductive, then wrap one end of the copper wire around one side of the polished pencil lead and fix it with a 1:1 mixture of AB glue.

[0113] In step 1.2, the volume ratio of nitric acid to water in the nitric acid aqueous solution is 1:1.5; and the ultrasonic cleaning time is 8 minutes.

[0114] The cut length in step 1.3 is 1.5 cm.

[0115] Step 2, preparation of electrolyte;

[0116] Step 2 is implemented as follows:

[0117] Prepare 500 ml of 0.5 mol / L sulfuric acid solution: measure 13.38 ml of sulfuric acid, add enough distilled water, dilute and make up to 500 ml in a volumetric flask;

[0118] Prepare 250 ml of 0.2 mol / L pyrrole solution: weigh 3.35 g of pyrrole, add distilled water to dissolve, and then dilute to 250 ml.

[0119] Prepare 250 ml of 0.3 mol / L potassium sulfate solution: weigh 13.07 g potassium sulfate, dissolve it in deionized water, and dilute to 250 ml in a volumetric flask.

[0120] Step 3: Preparation of working electrode.

[0121] Step 3 is implemented as follows:

[0122] Step 3.1, preparation of polypyrrole electrode: select a pencil lead with a length of 1.5 cm as the electrode substrate, ensure that its surface is clean and free of impurities, immerse the pencil lead electrode in the electrolyte, perform electrochemical polymerization using cyclic voltammetry CV, and scrape off the surface of the pencil lead after drying to obtain polypyrrole;

[0123] Step 3.2, preparation of bamboo charcoal / polypyrrole electrode: Soak the pencil core electrode in bamboo charcoal dispersion solution for 12 minutes to obtain a bamboo charcoal / pencil core electrode, place it in an electrolyte with a pyrrole concentration of 0.2 mol / L, a K2SO4 concentration of 0.3 mol / L, and a H2SO4 concentration of 0.5 mol / L, and use cyclic voltammetry CV to perform electrochemical polymerization. After drying, scrape it from the surface of the pencil core to obtain bamboo charcoal / polypyrrole.

[0124] The electrolyte in step 3.1 has a pyrrole concentration of 0.2 mol / L, a K2SO4 concentration of 0.3 mol / L, and a H2SO4 concentration of 0.5 mol / L;

[0125] When cyclic voltammetry (CV) is used for electrochemical polymerization in step 3.1, the scan rate is set to 0.3 V / s, and 9 cycles are scanned within the potential range of 0.2 V.

[0126] The concentration of the bamboo charcoal dispersion solution in step 3.2 is 5 mg / ml, and the immersion time is 10 min.

[0127] In order to optimize the preparation conditions of the conductive material, the present invention designed a systematic orthogonal experimental scheme. In the experiment, four key factors were considered: the effective length of the substrate electrode, the enrichment time of bamboo charcoal, the pH value of the electrolyte (the electrolyte for preparing the electrode), and the concentration of potassium chloride (the electrolyte for testing the charge). Each factor was set at three different levels to comprehensively evaluate their effects on the electrochemical properties of the material.

[0128] Test method for charge of polypyrrole and bamboo charcoal / polypyrrole:

[0129] Prepare the supporting electrolyte (0.1mol / L KCL+0.2mol / L H2SO4) and let it stand for 10 minutes before testing.

[0130] The polypyrrole / pencil lead is connected to the working electrode in the three-electrode system to form a complete detection circuit and is used together with the reference electrode and the auxiliary electrode. The charge test data of a single polypyrrole is obtained by continuously scanning 2 circles (4 scanning segments) at -0.1-0.6V at a scanning rate of 0.03V / s.

[0131] The working electrodes in the polypyrrole / bamboo charcoal / pencil lead three-electrode system are connected to form a complete detection circuit and used together with the reference electrode and the auxiliary electrode. The basic data of the charge of bamboo charcoal / polypyrrole are obtained by continuously scanning 2 circles (4 segments) at -0.1-0.6V at a scanning rate of 0.03V / s.

[0132] Select 3-4 segments from the scanning segments of the cyclic voltammetry of polypyrrole and bamboo charcoal / polypyrrole and import them into origin to calculate the absolute area of ​​the surrounded graph, and then calculate the charge according to formula 1.

[0133] Q = ∫I dl dt (1)

[0134] Bamboo charcoal concentration selection:

[0135] In this experiment, a single factor method was applied to determine the effect of different concentrations of bamboo charcoal on the polymer morphology of the modified electrode surface, and how this effect acts on the polymerization behavior of pyrrole on the bamboo charcoal / graphite electrode.

[0136] The effect of bamboo charcoal concentrations ranging from 1 mg / ml to 9 mg / ml on the charge in cyclic voltammetry curves was studied in a 0.07 mol / L pyrrole solution with an electrolyte of pH 0.4. Figure 1 It is known that in the bamboo charcoal concentration range of 1mg / ml to 5mg / ml, the charge on the electrode surface shows a significant growth trend. However, when the bamboo charcoal concentration exceeds 5mg / ml, the growth of the charge tends to a stable state. Based on these experimental results, the bamboo charcoal concentration of 5mg / ml is determined to be the optimal condition for achieving the best polymerization effect. Orthogonal experiment selects the best preparation conditions for polypyrrole:

[0137] Factor selection and orthogonal array selection:

[0138] An orthogonal design experimental method was used to evaluate the effects of four key factors on the charge during electrochemical polymerization. The selected factors included: pyrrole concentration level (0.03 mol / L, 0.05 mol / L, 0.07 mol / L, respectively), potential scanning rate (0.03 V / s, 0.05 V / s, 0.07 V / s, respectively), potential scanning range (0-0.6 V, -0.1-0.6 V, -0.2-0.6 V, respectively), and scanning number (8, 10, 12, respectively). As shown in Table 1, through this four-factor three-level experimental scheme, it is hoped that with the minimum number of experiments, how these factors independently and interactively affect the preparation of bamboo charcoal / polypyrrole composites can be systematically studied.

[0139] Table 1 Four-factor three-level orthogonal table

[0140]

[0141] After the four-factor three-level table was established, the standard experimental conditions were obtained through orthogonal experimental analysis and bamboo charcoal / polypyrrole composite materials were prepared under these conditions. Cyclic voltammetry was performed in an electrolyte of 0.1 mol / L KCL to scan four fragments and select 3-4 fragments. The data were imported into origin to calculate the area enclosed by the image (representing the charge) as shown in Table 2.

[0142] Table 2 Orthogonal experiment table

[0143]

[0144] Using orthogonal design experimental software, the experimental data were analyzed in detail, and the mean and range were obtained. The results are shown in Table 3. By corresponding the four factors (pyrrole concentration; scanning speed; scanning range; and scanning number) to columns 1, 2, 3, and 4 of Table 3, the three levels (such as pyrrole concentration 0.03mol / L; 0.05mol / L; 0.07mol / L) correspond to mean 1, mean 2, and mean 3 of Table 3. If the mean 3 in the first column is the largest, the optimal concentration is 0.07mol / L. By analogy, the optimal conditions for preparing bamboo charcoal / polypyrrole composite materials were determined. These conditions include: the concentration of pyrrole is 0.07mol / L, the potential scanning rate is 0.03V / s, the potential scanning range is selected as -0.1-0.6V, and the number of scanning circles is fixed to 8 circles.

[0145] Table 3 Analysis results obtained by orthogonal experimental analysis

[0146] Serial number 1 2 3 4 Mean 1 3.203 3.897 2.957 4.133 Mean 2 3.210 3.823 4.080 3.863 Mean 3 4.177 2.870 3.553 2.593 Very bad 0.947 1.027 1.123 1.504

[0147] Four other key factors were also considered: the effective length of the substrate electrode, the enrichment time of bamboo charcoal, the pH value of the electrolyte (electrolyte for preparing the electrode), and the concentration of potassium chloride (electrolyte for testing the charge). Each factor was set at three different levels (Table 4) to fully evaluate their effects on the electrochemical performance of the material.

[0148] Table 4 Four-factor three-level orthogonal table

[0149]

[0150]

[0151] Nine groups of electrodes with different conditions were prepared according to Table 4, and orthogonal experiments were carried out under the conditions of pyrrole concentration of 0.07 mol / L, potential scanning rate of 0.03 V / s, potential scanning range of -0.1-0.6 V, and scanning number of 8 circles. The orthogonal experiment table is shown in Table 5.

[0152] Table 5 Orthogonal experiment table

[0153]

[0154] Through the experiment, we get nine groups of experimental data as follows Figure 2 shown.

[0155] Import the data into the origin software and use the integration tool to get the relative integrated area. According to formula (1),

[0156] The charge is calculated and the data are shown in Table 6.

[0157] Table 6 Orthogonal experimental data

[0158]

[0159]

[0160] Taking charge as the measurement index, the four factors are analyzed, see Table 7.

[0161] Table 7 Orthogonal experimental data analysis

[0162]

[0163] The results of the orthogonal experiment were analyzed. The level mean represents the average level of the experimental results under the level condition. The larger the level mean, the better the experimental results under the level condition. The range represents the degree of influence of the factor on the experimental results. The larger the range, the greater the influence of the change of the factor on the experimental results. The level 3 mean of the factor electrode length is the largest (28.80), so the condition represented by level 3 is the best condition for this factor. According to the corresponding relationship of the level factors in Table 4, the condition represented by level 3 under the electrode length is that the electrode length is 1.50cm, so the optimal length of the prepared electrode is 1.50cm. Similarly, the optimal time for bamboo charcoal enrichment is 15min, the optimal pH value of the electrolyte (electrolyte for preparing the electrode) is 0.10, and the optimal concentration of potassium chloride (electrolyte for testing the charge) is 0.2mol / L.

[0164] Experimental Section

[0165] Experimental equipment:

[0166] In this experiment, cyclic voltammetry and a three-electrode working system were used. Figure 3 The electrochemical test was performed as shown in the figure. The working electrode was a homemade bamboo charcoal / pencil lead (BC / PEC) modified electrode, the reference electrode was a saturated calomel electrode (SCE), and the auxiliary electrode was a platinum electrode.

[0167] Preparation of bamboo charcoal / polypyrrole composite materials:

[0168] Prepare the supporting electrolyte (composition: 0.2mol / L H2SO4+0.1mol / L K2SO4+0.07mol / L pyrrole) and let it stand for 10 minutes before testing.

[0169] The pencil core electrode (PEC) is connected to the working electrode of the three-electrode system to form a complete detection circuit and is used together with the reference electrode and the auxiliary electrode. Single polypyrrole is obtained by continuous scanning at -0.1-0.6V at a scanning rate of 0.03V / s for 8 cycles.

[0170] The working electrode of the modified electrode (BC / PEC) three-electrode system is connected to form a complete detection circuit and used together with the reference electrode and the auxiliary electrode. Bamboo charcoal / polypyrrole is obtained by continuous scanning at -0.1-0.6V at a scanning rate of 0.03V / s for 8 cycles.

[0171] Preparation process of polypyrrole and bamboo charcoal / polypyrrole:

[0172] As shown in Figure 4(a) and Figure 4(b), multi-scan cyclic voltammetry curves of polypyrrole and bamboo charcoal / polypyrrole composites prepared under the optimal conditions (pyrrole concentration 0.07 mol / L; scan rate 0.03 V / s; scan range -0.1-0.6 V; scan number 8 circles) in the electrochemical polymerization supporting electrolyte (0.01 mol / L K2SO4+0.2 mol / LH2SO4) with a pH of 0.4.

[0173] The peak current, peak potential and charge data of Figure 4(a) and Figure 4(b) are tabulated as shown in Table 8:

[0174] Table 8 Peak current, peak potential and charge data table

[0175]

[0176]

[0177] After a detailed analysis of the cyclic voltammetry (CV) characteristics of polypyrrole and bamboo charcoal / polypyrrole composites, it was found that the addition of bamboo charcoal had no significant effect on the peak current and peak potential. However, when comparing the charge storage capacity of the two materials, a significant difference was found: in the bamboo charcoal / polypyrrole composite, the charge was significantly increased compared to pure polypyrrole. This shows that the introduction of bamboo charcoal significantly enhances the charge storage performance of the material.

[0178] The prepared samples were dried as shown in Figure 5(a) and Figure 5(b) for subsequent inspection. Figure 5(a) shows pure polypyrrole scraped from a pencil lead, and Figure 5(b) shows a bamboo charcoal / polypyrrole composite material scraped from a bamboo charcoal / pencil lead.

[0179] Constant current charge and discharge test (GCD) comparison:

[0180] In the right Figure 6 After detailed analysis of the constant charge and discharge test (GCD) curve shown in Figure 1 (parameters: cathode current and anode current are 0.005A; minimum potential is 0V, maximum potential is 1.2V; scan 4 segments), it is found that the charge and discharge time of single polypyrrole is 27.5s, and the corresponding constant voltage difference is 0.591V. In contrast, the charge and discharge time of bamboo charcoal / polypyrrole composite material is extended to 38s, and its constant voltage difference is increased to 0.712V. This shows that the addition of bamboo charcoal improves the electrochemical performance of polypyrrole, which is reflected in longer charge and discharge time and higher voltage maintenance ability. It may be due to the high conductivity and excellent structural stability of bamboo charcoal, which act together on the electrode material, thereby improving its overall electrochemical energy storage performance.

[0181] Depend on Figure 6The data from the constant charge and discharge current test can be used to calculate the specific capacitance of the two materials according to Formula 2. C is the specific capacitance: F / g; m is the active substance of the electrode material: g; Δt is the discharge time: s; ΔV is the voltage during discharge: V.

[0182]

[0183] Table 9 GCD test data and charge calculation table

[0184]

[0185] By analyzing the data in Table 9, it can be observed that the specific capacitance of the bamboo charcoal / polypyrrole composite material is 266.853 (F / g), while the specific capacitance of single polypyrrole is 233.657 (F / g). The specific capacitance of the bamboo charcoal / polypyrrole composite material is higher than that of single polypyrrole, indicating that the introduction of bamboo charcoal improves the energy storage performance of polypyrrole. The increase in specific capacitance is due to the high conductivity and excellent pore structure of bamboo charcoal, which provides more active sites and faster electron migration paths for charge storage and transmission. Therefore, the bamboo charcoal / polypyrrole composite material shows better performance than single polypyrrole in the field of electrochemical energy storage.

Claims

1. A method for preparing a bamboo charcoal modified polypyrrole composite material, characterized in that: Follow the steps below to implement it: Step 1, preparation of substrate electrode; Step 2, preparation of electrolyte; Step 3: Preparation of working electrode.

2. The method for preparing the bamboo charcoal modified polypyrrole composite material according to claim 1, characterized in that: The step 1 is specifically implemented according to the following steps: Step 1.1, take out the lead of a 2B pencil and cut it into small pieces of 1-2.0 cm, use sandpaper to smooth both sides of the small piece of pencil lead and ensure that the effective length is the required length; Step 1.2, the small pencil lead after step 1.1 is ultrasonically cleaned in nitric acid aqueous solution and distilled water for 10 minutes respectively to remove impurities, taken out and dried for later use; Step 1.3, polish the surface of the pencil lead that has been dried in step 1.2, cut a length of enameled copper wire, remove the enameled film on the surface of the copper wire by soaking it in sulfuric acid, and process it until the copper wire is exposed at both ends to make it conductive, then wrap one end of the copper wire around one side of the polished pencil lead and fix it with a 1:1 mixture of AB glue.

3. The method for preparing the bamboo charcoal modified polypyrrole composite material according to claim 2, characterized in that: In the step 1.2, the volume ratio of nitric acid to water in the nitric acid aqueous solution is 1:1 to 1:2; and the ultrasonic cleaning time is 5 to 15 minutes.

4. The method for preparing the bamboo charcoal modified polypyrrole composite material according to claim 2, characterized in that: The intercepted length in step 1.3 is 1-2 cm.

5. The method for preparing the bamboo charcoal modified polypyrrole composite material according to claim 2, characterized in that: The step 2 is specifically implemented according to the following steps: Prepare 250-1000 ml of 0.1-1 mol / L sulfuric acid solution, 250-500 ml of 0.1-0.3 mol / L pyrrole solution, and 500-1000 ml of 0.05-0.6 mol / L potassium sulfate solution respectively.

6. The method for preparing the bamboo charcoal modified polypyrrole composite material according to claim 3, characterized in that: The step 3 is specifically implemented according to the following steps: Step 3.1, preparation of polypyrrole electrode: select a pencil lead with a length of 1-2 cm as the electrode substrate, ensure that its surface is clean and free of impurities, immerse the pencil lead electrode in an electrolyte, perform electrochemical polymerization using cyclic voltammetry CV, and scrape off the surface of the pencil lead after drying to obtain polypyrrole; Step 3.2, preparation of bamboo charcoal / polypyrrole electrode: soak the pencil core electrode in bamboo charcoal dispersion solution to obtain bamboo charcoal / pencil core electrode, place it in electrolyte with pyrrole concentration, K SO concentration, and H SO concentration, perform electrochemical polymerization by cyclic voltammetry (CV), and scrape off the surface of the pencil core after drying to obtain bamboo charcoal / polypyrrole.

7. The method for preparing the bamboo charcoal modified polypyrrole composite material according to claim 6, characterized in that: In the electrolyte in step 3.2, the concentration of pyrrole is 0.1-0.3 mol / L, the concentration of K SO is 0.05-0.6 mol / L, and the concentration of H SO is 0.1-1 mol / L.

8. The method for preparing the bamboo charcoal modified polypyrrole composite material according to claim 6, characterized in that: When cyclic voltammetry (CV) is used for electrochemical polymerization in step 3.1, the scan rate is set to 0.01-0.5 V / s, and 4-16 cycles of scanning are performed in the potential range of -0.1 V to 0.6 V, 0 V to 0.6 V, and -0.2 to 0.6 V.

9. The method for preparing the bamboo charcoal modified polypyrrole composite material according to claim 6, characterized in that: The concentration of the bamboo charcoal dispersion solution in step 3.2 is 1-9 mg / ml, and the soaking time is 5-20 min.

10. The bamboo charcoal modified polypyrrole composite material prepared by the method for preparing the bamboo charcoal modified polypyrrole composite material according to any one of claims 1 to 9.