Ferrozirconium red pigment produced from zircon powder and production method thereof
By performing high-temperature melting, alkali-soluble and liquid-phase reaction treatment on zircon powder, the stability problem of zircon powder in synthesis of zircon iron red material is solved, and the low-cost production of zircon iron red material is achieved, and the high-active electricity production is replaced. Melting zirconia or chemical zirconium reduces production costs and maintains coloring effect.
Patent Information
- Application Number
- CN202411011478.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-22
AI Technical Summary
At present, the ceramic coloring industry mainly uses highly active electromelted zirconium oxide or chemical zirconium, resulting in high raw material costs. However, zircon powder cannot be used in coloring manufacturers due to its structural stability that does not meet the synthesis reaction conditions. Being widely used.
Zircon sand is melted at high temperature, cooled rapidly, and then crushed, placed in sodium hydroxide solution to dissolve, reacted with colorant, and then mixed with mineralizer for grinding and calcination to obtain a zirconium iron-red material.
This method changes the characteristics of zircon powder, so that it meets the requirements of zirconium iron red material synthesis reaction, can replace high-active electromelting zirconia or chemical zirconium, reduce production costs, and achieve the same color development effect as traditional methods.
Smart Images

Figure CN118994938A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ferrozirconium red material, and in particular to a ferrozirconium red material produced by using zircon powder and a production method thereof. Background Art
[0002] At present, the ceramic colorant industry uses highly active fused zirconium oxide or chemical zirconium to produce ferrozirconium red material. For example, the Chinese invention patent with publication number CN102173867A discloses a method for producing ferrozirconium red material with fused zirconium oxide. The fused zirconium oxide powder is first subjected to zirconium oxide powder crystal spheroidization treatment, washing and grinding, and then mixed with other raw materials for heating and calcining to obtain ferrozirconium red material. Using highly active fused zirconium oxide or chemical zirconium as raw materials has a high raw material cost. Although zircon powder has a relatively advantageous price, no colorant manufacturer currently uses zircon powder to make ferrozirconium red material, mainly because zircon powder has a stable structure and does not meet the conditions for the synthesis reaction of ferrozirconium red material. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a zirconium iron red material produced by using zircon powder and a production method thereof.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for producing red zirconium iron material using zircon powder, comprising the following steps:
[0005] S1: melting zircon sand, cooling it, and then crushing it into particles;
[0006] S2: placing the particles in a sodium hydroxide solution for dissolution;
[0007] S3: adding a colorant solution dropwise to the dissolved solution to react and obtain a product;
[0008] S4: The product is washed and mixed with a mineralizer, and then ground and calcined in sequence to obtain a zirconium iron red material.
[0009] Another technical solution adopted by the present invention is: a zirconium iron red material is produced by adopting the above production method.
[0010] The beneficial effects of the present invention are as follows: the production method of the present invention makes zircon sand meet the requirements of the synthesis reaction of ferrozirconium red material by subjecting zircon powder to treatment methods such as melting, alkali dissolution and liquid phase reaction, and can replace high-activity fused zirconium oxide or chemical zirconium to produce ferrozirconium red material, thereby reducing the production cost of ferrozirconium red material. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 Shown is a process flow chart of Example 1 of the present invention. DETAILED DESCRIPTION
[0012] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in combination with the implementation modes and the accompanying drawings.
[0013] A method for producing red ferrozirconium material using zircon powder comprises the following steps:
[0014] S1: melting zircon sand, cooling it, and then crushing it into particles;
[0015] S2: placing the particles in a sodium hydroxide solution for dissolution;
[0016] S3: adding a colorant solution dropwise to the dissolved solution to react and obtain a product;
[0017] S4: The product is washed and mixed with a mineralizer, and then ground and calcined in sequence to obtain a zirconium iron red material.
[0018] From the above description, it can be seen that the beneficial effect of the present invention is that: the production method of the present invention uses S1 to S3 to sequentially perform melting, alkali dissolution and liquid phase reaction with a colorant on zircon powder, thereby effectively changing the original properties of zircon sand to meet the requirements of the synthesis reaction of ferrozirconium red material, and can completely replace high-activity fused zirconium oxide or chemical zirconium to produce ferrozirconium red material, thereby reducing the production cost of ferrozirconium red material.
[0019] Furthermore, the melting temperature in S1 is 2300-2500°C.
[0020] From the above description, it can be seen that when the melting temperature is lower than 2300°C, the zircon sand melting effect is poor; when it is higher than 2500°C, the smelting cost increases; therefore, the present invention controls the melting temperature to be 2300-2500°C, the zircon sand can be completely melted, and the melt has good fluidity.
[0021] Furthermore, the specific step of cooling in S1 is: spraying the molten zircon sand into a device filled with water for rapid cooling to obtain hollow spherical zircon sand.
[0022] From the above description, it can be seen that the conventional cooling method is mostly natural cooling, and the particles cooled naturally are solid, which is not convenient for subsequent processing.
[0023] Furthermore, the size of the particles in S1 is 300-350 mesh.
[0024] Furthermore, after iron is removed from the particles in S1, step S2 is performed.
[0025] From the above description, it can be seen that the purpose of iron removal is to remove the mechanical iron in the particles to avoid affecting the color tone of the subsequent ferrozirconium red material.
[0026] Furthermore, the specific step of S2 is: placing the particles in a sodium hydroxide solution with a mass concentration of 20 to 30% under a pressure of 1 to 3 MPa to dissolve them, and then passing them through a sieve of 50 to 80 meshes for later use.
[0027] From the above description, it can be seen that during the alkaline dissolution process, when the pressure is lower than 1 MPa, the alkaline dissolution effect is poor and insoluble matter will appear; the present invention controls the alkaline dissolution to be carried out under a pressure of 1 to 3 MPa, so that the product in S1 can be completely dissolved.
[0028] Under the same pressure conditions, the lower the concentration of the sodium hydroxide solution, the lower the product dissolution efficiency in S1; too high a concentration of the sodium hydroxide solution will increase the processing cost.
[0029] Furthermore, after the reaction in S3, sulfuric acid with a mass concentration of 3 to 5% is used to control the pH of the product to be 8.5 to 9.5.
[0030] From the above description, it can be seen that when the pH value is lower than 8.5, silica will be lost, affecting the subsequent colorant reaction effect; when the pH value is higher than 9.5, it will increase the difficulty of cleaning treatment in subsequent processes, and the residue will affect the reaction temperature of the colorant, resulting in a worse coloring effect.
[0031] Furthermore, the colorant solution in S3 includes a soluble iron salt.
[0032] Furthermore, the soluble iron salt is ferric sulfate or ferrous sulfate.
[0033] From the above description, it can be seen that the residual sulfate has no adverse effect on the reaction of zirconium iron red material, and the residual ions in other iron salts have an adverse effect on the reaction of zirconium iron red material; therefore, the soluble iron salt is specifically selected to be ferric sulfate or ferrous sulfate.
[0034] Furthermore, the colorant solution includes a soluble iron salt and water, and the mass ratio of the soluble iron salt to the water is 1:3-5.
[0035] Furthermore, the mineralizer in S4 includes sodium fluoride and magnesium fluoride.
[0036] From the above description, it can be seen that the mineralizers in the present invention mainly use sodium fluorosilicate and magnesium fluoride. This mineralizer composition can make the colorant loose after calcination, and the colorant reaction effect is good and the coloring power is strong. If other mineralizers are used, the colorant is easy to harden, which affects the coloring effect of the zircon red material.
[0037] Furthermore, the specific steps of washing in S4 are: washing the product with 3 to 5 times of water for 2 to 3 times, and then drying at 150 to 200° C. to control the water content within 0.5%.
[0038] Furthermore, the calcination in S4 is specifically as follows: uniformly heating to 1030-1080° C. within 3-5 hours, and keeping the temperature for 1-2 hours.
[0039] From the above description, it can be seen that if the heating time during calcination is less than 3 hours, the colorant will be under-burned, the colorant will not react fully and the coloring effect will be affected; if the heating time is more than 5 hours, the calcination cost will increase; if the insulation time is too long, the zirconium silicate crystals will be too large, which will reduce the coloring power of the colorant and increase the calcination cost.
[0040] Another technical solution adopted by the present invention is: a zirconium iron red material is produced by adopting the above production method.
[0041] Please refer to Figure 1 Embodiment 1 of the present invention is: a method for producing red ferrozirconium material using zircon powder, the steps are as follows:
[0042] S1. High temperature melting treatment: zircon sand is placed in an electric arc furnace, melted at 2400°C, and then sprayed into a device filled with water for rapid cooling to obtain zircon sand in the shape of a hollow sphere.
[0043] S2. Particle crushing: The hollow spherical zircon sand is crushed into 325 mesh particles by Raymond mill, and the particle size is controlled by a laser particle size analyzer; then the particles are de-ironized by a dry magnetic separator and set aside.
[0044] S3, alkali dissolution treatment: weigh 500g of the iron-removed particles, weigh 200g of sodium hydroxide and prepare a sodium hydroxide solution with a mass concentration of 25%, put the two in a reactor, dissolve under a pressure of 2MPa, and then pass through a 60-mesh sieve for use.
[0045] S4, colorant reaction treatment: weigh 200 g of ferrous sulfate, use 1000 mL of industrial aqueous solution to obtain a colorant solution; react with the solution obtained by dissolving in S3 by titration to obtain a product; then use sulfuric acid with a mass concentration of 4% to control the pH of the product to 9.
[0046] S5. Cleaning treatment: The product with pH 9 in S4 is washed twice with 1000 mL of water, and then dried at 170° C. for later use, wherein the water content of the dried product is controlled to be about 0.3%.
[0047] S6, calcination treatment: weigh the product after washing and drying in S5, mix it evenly with a mineralizer to obtain a mixture, the mineralizer includes sodium fluorosilicate and magnesium fluoride, the proportion of sodium fluorosilicate in the mixture is 1.5wt%, and the proportion of magnesium fluoride in the mixture is 1.5wt%; uniformly heat the mixture to 1050°C within 4 hours, keep it warm for 1.5 hours, cool it down and take it out to obtain zirconium iron red material.
[0048] S7. Prepare the sample: grind the red ferrozirconium material with a weight ratio of material: ball: water = 1:3:0.5 for 4 minutes; then wash it with water twice, and the weight ratio of slurry: water during washing is 1:20; finally dry it at a drying temperature of 150°C, and the water content after drying is controlled to be 0.3% to obtain the sample. The color of the red ferrozirconium material of the sample is compared with the zirconium oxide standard product, and the comparison results are shown in Table 1.
[0049] Table 1
[0050]
[0051] As shown in Table 1, the color development test results show that the color development of the zircon red material prepared by using zircon sand in the present invention reaches or exceeds the color development effect of the zircon red zircon oxide standard sample.
[0052] The method for producing ferrozircon red of the present invention is different from the traditional production method. It directly utilizes the silicon dioxide in zircon sand to participate in the colorant reaction. The traditional method requires desiliconization of zircon sand or chemical conversion into zirconium dioxide before adding silicon dioxide. The method of the present invention reduces the processing cost and material cost of the desiliconization link, saving about 3,000 yuan in processing and material costs per ton of colorant; in addition, the method reduces the long-term grinding process of the traditional semi-finished colorant, saving about 2,000 yuan in grinding costs per ton of colorant.
[0053] Embodiment 2 of the present invention is: a method for producing red zirconium iron material using zircon powder, the steps are as follows:
[0054] S1. High temperature melting treatment: zircon sand is placed in an electric arc furnace, melted at 2300°C, and then sprayed into a device filled with water for rapid cooling to obtain zircon sand in the shape of a hollow sphere.
[0055] S2. Particle crushing: The hollow spherical zircon sand is crushed into 300-mesh particles using a Raymond mill, and the particle size is controlled by a laser particle size analyzer; then the particles are de-ironized using a dry magnetic separator for later use.
[0056] S3, alkali dissolution treatment: weigh 500g of the iron-removed particles, weigh 200g of sodium hydroxide and prepare a sodium hydroxide solution with a mass concentration of 20%, put the two in a reactor, dissolve under a pressure of 1MPa, and then pass through a 50-mesh sieve for use.
[0057] S4, colorant reaction treatment: weigh 200 g of ferrous sulfate, use 600 mL of industrial aqueous solution to obtain a colorant solution; react with the solution obtained by dissolving in S3 by titration to obtain a product; then use sulfuric acid with a mass concentration of 3% to control the pH of the product to 8.5.
[0058] S5. Cleaning treatment: The product with a pH of 8.5 in S4 is washed three times with 1000 mL of water, and then dried at 150° C. for later use, wherein the water content of the dried product is controlled to be about 0.3%.
[0059] S6. Calcination treatment: weigh the product after washing and drying in S5, mix it evenly with a mineralizer and grind it to obtain a mixture, the mineralizer includes sodium fluorosilicate and magnesium fluoride, the proportion of sodium fluorosilicate in the mixture is 1.5wt%, and the proportion of magnesium fluoride in the mixture is 1.5wt%; uniformly heat the mixture to 1030°C within 3h, keep it warm for 2h, cool it down and take it out to obtain zirconium iron red material.
[0060] Embodiment 3 of the present invention is: a method for producing red zirconium iron material using zircon powder, the steps are as follows:
[0061] S1. High temperature melting treatment: zircon sand is placed in an electric arc furnace, melted at 2500°C, and then sprayed into a device filled with water for rapid cooling to obtain zircon sand in the shape of a hollow sphere.
[0062] S2. Crushing and iron removal: The hollow spherical zircon sand is crushed into 350 mesh particles by Raymond mill, and the particle size is controlled by a laser particle size analyzer; then the particles are iron-removed by a dry magnetic separator for later use.
[0063] S3, alkali dissolution treatment: weigh 500g of the iron-removed particles, weigh 200g of sodium hydroxide and prepare a sodium hydroxide solution with a mass concentration of 30%, put the two in a reactor, dissolve under a pressure of 3MPa, and then pass through a 80-mesh sieve for use.
[0064] S4, colorant reaction treatment: weigh 200 g of ferrous sulfate, use 800 mL of industrial aqueous solution to obtain a colorant solution; react with the solution obtained by dissolving in S3 by titration to obtain a product; then use sulfuric acid with a mass concentration of 5% to control the pH of the product to 9.5.
[0065] S5. Cleaning treatment: The product with a pH of 9.5 in S4 is washed with 1000 mL of water, and then dried at 200° C. for later use, wherein the water content of the dried product is controlled to be about 0.3%.
[0066] S6, calcination treatment: weigh the product after washing and drying in S5, mix it evenly with a mineralizer and grind it to obtain a mixture, the mineralizer includes sodium fluorosilicate and magnesium fluoride, the proportion of sodium fluorosilicate in the mixture is 1.5wt%, and the proportion of magnesium fluoride in the mixture is 1.5wt%; the mixture is uniformly heated to 1080°C within 5 hours, kept warm for 1 hour, cooled and taken out to obtain zirconium iron red material.
[0067] In summary, the zircon red material produced by zircon powder and the production method thereof provided by the present invention change the original properties of zircon sand by modifying zircon sand, so that it can be used for the synthesis reaction of zircon red material. The method of the present invention is used to replace the existing fused zirconium oxide or chemical zirconium to produce zircon red material, which can reduce the production cost.
[0068] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's specification and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for producing red zirconium iron material using zircon powder, characterized in that: The following steps are involved: S1: melting zircon sand, cooling it, and then crushing it into particles; S2: placing the particles in a sodium hydroxide solution for dissolution; S3: adding a colorant solution dropwise to the dissolved solution to react and obtain a product; S4: The product is washed and mixed with a mineralizer, and then ground and calcined in sequence to obtain a zirconium iron red material.
2. The method for producing red zirconium iron material using zircon powder according to claim 1, characterized in that: The melting temperature in S1 is 2300-2500°C.
3. The method for producing red zirconium iron material using zircon powder according to claim 1, characterized in that: The specific step of cooling in S1 is to spray the molten zircon sand into a device filled with water for rapid cooling to obtain hollow spherical zircon sand.
4. The method for producing red zirconium iron material using zircon powder according to claim 1, characterized in that: The size of the particles in S1 is 300-350 meshes.
5. The method for producing red zirconium iron material using zircon powder according to claim 1, characterized in that: After the iron is removed from the particles in S1, step S2 is performed.
6. The method for producing red zirconium iron material using zircon powder according to claim 1, characterized in that: The specific steps of S2 are: placing the particles in a sodium hydroxide solution with a mass concentration of 20-30% under a pressure of 1-3 MPa to dissolve them, and then passing them through a sieve with a mesh size of 50-80 for later use.
7. The method for producing red zirconium iron material using zircon powder according to claim 1, characterized in that: After the reaction in S3, sulfuric acid with a mass concentration of 3 to 5% is used to control the pH of the product to be 8.5 to 9.
5.
8. The method for producing red zirconium iron material using zircon powder according to claim 1, characterized in that: The colorant solution in S3 includes a soluble iron salt.
9. The method for producing red zirconium iron material using zircon powder according to claim 1, characterized in that: The mineralizer in S4 includes sodium fluoride and magnesium fluoride.
10. A zirconium iron red material, characterized in that: The product is produced by the production method described in any one of claims 1 to 9.
Citation Information
Patent Citations
Process for producing ferrozirconium red material
CN101429053A
Preparation method of zirconium silicon black ceramic pigment
CN103396161A
Production method of high-activity fused zirconia
CN110683578A
Method for producing ferrozirconium red pigment for ceramic ink from fused zirconia
CN117946540A
Method for joint production of hexafluorozirconic acid and silicon tetrafluoride
CN118084053A