Impact-resistant polyester resin powder coating and preparation method thereof
By adding modified polyurethane elastomer and reinforced filler to the polyester resin powder coating, the problem of insufficient heat resistance and impact resistance of polyester powder coating is solved, and higher coating toughness and corrosion resistance are achieved, improving The overall performance of the material.
Patent Information
- Application Number
- CN202411183541.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
AI Technical Summary
The thermal resistance, impact resistance and corrosion resistance of polyester powder coatings on the market are poor, resulting in the coating being easily damaged and corroded when impacted by external forces, affecting its use and aesthetics.
Using polyester resin as the matrix, modified polyurethane elastomer and reinforced filler are added, and modified polyurethane elastomer and reinforced filler are prepared through specific synthesis steps to improve the toughness and mechanical properties of the coating, and benzimidazole and vinyl trimethyl Compounds such as oxysilane form intermediates, and are modified with nanoalumina and chitosan to form SiO2@Al2O3 nanomaterials, enhancing the dispersion and corrosion resistance of the filler.
It significantly improves the impact resistance, heat resistance and corrosion resistance of powder coatings, enhances the toughness and mechanical properties of the coating, prevents the coating from rupturing and corrosion during external impact, and improves the durability of the material.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyester resin powder coatings, and in particular to an impact-resistant polyester resin powder coating and a preparation method thereof. Background Art
[0002] Powder coating is a kind of coating that does not contain organic solvents, is applied in powder form and cured by baking to form a film. Compared with traditional solvent-based coatings, powder coatings have the advantages of high efficiency and energy saving, green environmental protection, simple process and high utilization rate. Therefore, they have been widely used in the fields of construction, home appliances, engineering machinery, etc. Powder coatings are divided into two categories: thermoplastic and thermosetting. The film appearance of thermoplastic powder coatings is poor and the adhesion between them and metal is also poor; thermosetting powder coatings use thermosetting synthetic resin as the film-forming material. During the drying process, the resin first melts and then solidifies into a flat and hard coating film after chemical cross-linking. The polyester powder coatings currently on the market have poor heat resistance, impact resistance and corrosion resistance. For example, the surface of the coating is easily impacted by external forces during daily use, which will cause damage and cracking of the coating, affecting the normal use and aesthetics of the coating.
[0003] In view of the shortcomings of powder coatings, they can be modified, for example: by adding nanofillers or toughening agents to increase the toughness and impact strength of the coating and improve the impact resistance; by introducing corrosion-resistant substances (polyaniline, chitosan, etc.) to improve the corrosion resistance of the coating; by adding fillers or polymers with good heat resistance to improve the heat resistance of the coating. Based on the above modification methods, researchers have developed a powder coating based on polyester resin to improve the impact resistance, heat resistance and corrosion resistance of the coating. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides an impact-resistant polyester resin powder coating and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions: An impact-resistant polyester resin powder coating comprises the following raw materials in parts by weight: 55-75 parts of polyester resin, 5-9 parts of curing agent, 7-10 parts of modified polyurethane elastomer, 10-20 parts of reinforcing filler, 1-3 parts of antioxidant, 2-3 parts of dispersant, and 0.5-2 parts of leveling agent; The modified polyurethane elastomer is prepared by the following steps: Step A1: benzimidazole, anhydrous ethanol and vinyltrimethoxysilane are mixed, nitrogen is introduced, reacted, and rotary evaporated to obtain an intermediate; Step A2: Under nitrogen, dimethyldiethoxysilane, dimethylethoxysilane, N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane, the intermediate and solution 1 are mixed for reaction, the product is collected, cyclohexane and 732 cation exchange resin are added in sequence, stirred, filtered and distilled to obtain amino-containing organosilicon; Step A3: After dehydrating the polyethylene glycol in vacuo, argon is introduced, isophorone diisocyanate and dibutyltin dilaurate are added to react, and then toluene, amino-containing silicone and ethylenediamine are added to react to obtain a modified polyurethane elastomer.
[0006] Furthermore, in step A1, the dosage ratio of benzimidazole, vinyltrimethoxysilane and anhydrous methanol is 0.1 mol: 0.12-0.2 mol: 100 mL, the reaction temperature in step A1 is 35° C., and the reaction time is 3-5 h.
[0007] Furthermore, in step A2, the mass ratio of dimethyldiethoxysilane, dimethylethoxysilane, N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane, intermediate, solution 1, cyclohexane and 732 cation exchange resin is 4.5:5.2-10.4:10.3-14.5:2.4-7.1:20:30:5-10. During the mixed reaction in step A2, the temperature is first raised to 55-65°C for reaction for 3-5h, and then raised to 120-130°C to remove alcohol and water. The stirring time after the addition of cyclohexane and 732 cation exchange resin is 10-30min and 20-40min, respectively.
[0008] Furthermore, in step A2, solution 1 is prepared by mixing potassium hydroxide, ethanol and deionized water in a mass ratio of 0.05-0.08:10:10.
[0009] Furthermore, in step A3, the dosage ratio of polyethylene glycol, isophorone diisocyanate, dibutyltin dilaurate, toluene, amino-containing silicone and ethylenediamine is 0.1 mol: 0.15-0.25 mol: 0.001-0.005 mol: 30-50 mL: 2-4 g: 3-6 g, the dehydration temperature of polyethylene glycol is 120-140° C., the time is 1-3 h, the reaction temperature of the elastomer is 70-90° C., and the two reaction times are 2-4 h and 2-3 h respectively.
[0010] The reinforcing filler is prepared by the following steps: Step B1: Add polyvinyl pyrrolidone to anhydrous ethanol and disperse it evenly, then add nano-alumina and ultrasonically disperse it for 30 minutes, slowly drop the mixed solution, and adjust the pH to 8.5-9, so that the mixed solution is added dropwise within 2-3 hours, and then continue to react at 35°C for 4 hours. After the reaction is completed, centrifuge, wash and dry to obtain SiO2@Al2O3 nanomaterials; Step B2: Disperse 1-3g of pre-treated chitosan in 10mL of deionized water, which is referred to as chitosan solution; add SiO2@Al2O3 nanomaterials to 1wt%-2wt% glutaraldehyde solution and disperse evenly, then raise the system temperature to 45°C to react for 30min, centrifuge and wash after the reaction is completed, then add chitosan solution, maintain the temperature and continue to react for 2-4h, centrifuge, wash and dry after the reaction is completed to obtain a reinforced filler; Furthermore, in step B1, the amount ratio of polyvinyl pyrrolidone, anhydrous ethanol, nano-alumina and the mixed solution is 2-4 g: 50 mL: 3 g: 10 mL, and the mixed solution is prepared by mixing ethyl orthosilicate, γ-aminopropyltriethoxysilane and anhydrous ethanol in an amount ratio of 0.1-0.2 g: 0.1 g: 10 mL; Further, in step B2, the amount ratio of SiO2@Al2O3 nanomaterial, glutaraldehyde solution and chitosan solution is 1 g: 20-30 mL: 10 mL; Furthermore, the pretreated chitosan in step B2 is prepared by the following steps: 5 g of chitosan is evenly dispersed in 10 mL of 2-3 wt% sodium hydroxide solution, and refrigerated at -10°C for 24 h, centrifuged after thawing, and the precipitate is dried at 60°C to obtain the pretreated chitosan.
[0011] A method for preparing an impact-resistant polyester resin powder coating comprises the following steps: The raw materials are weighed by weight, and each component of the raw materials is mixed and stirred evenly in a stirrer, and then melted, extruded, tableted, crushed, and sieved to obtain a powder with a particle size of 500-600 meshes to obtain an impact-resistant polyester resin powder coating.
[0012] Beneficial effects of the present invention: The powder coating of the present invention uses polyester resin as base resin, and is added with modified polyurethane elastomer and reinforcing filler, which work together to improve the impact resistance, heat resistance and corrosion resistance of the powder coating.
[0013] The modified polyurethane elastomer is firstly prepared by reacting the secondary amine in benzimidazole with the double bond in vinyltrimethoxysilane to generate an intermediate; then dimethyldiethoxysilane, dimethylethoxysilane, N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane and the intermediate are used as raw materials to synthesize amino-containing silicone; finally, polyethylene glycol, isophorone diisocyanate, amino-containing silicone and ethylenediamine are used as raw materials and dibutyltin dilaurate is used as a catalyst to synthesize the modified polyurethane elastomer. After the modified polyurethane elastomer is introduced into the coating, it can improve the toughness of the coating, make it have a certain impact resistance, and also improve the heat resistance of the substrate; the improvement of toughness is due to the active groups (Si-H bonds, -NCO groups) contained in the modified polyurethane elastomer can cross-link with the film-forming materials in the coating, thereby improving the strength and toughness of the coating. At the same time, the modified polyurethane elastomer has good dispersibility in the coating, which enables the coating to absorb part of the external mechanical energy when it is impacted to ensure that the coating is not damaged; after the amino-containing silicone is introduced into the elastomer as an amino chain extender, it is introduced into the main chain of the polyurethane molecule. The Si-O-Si structure is introduced to improve the mechanical properties of the elastomer, thereby improving the toughness and impact resistance of the coating. The amino chain extender can also react with the isocyanate group to form a urea bond, and hydrogen bonds can be formed between the urea bond and the carbamate. The strength of the hydrogen bond is relatively weak. When impacted by external force, the hydrogen bond can be broken and absorb part of the energy, thereby reducing stress concentration and preventing the coating from cracking. When the external force disappears, the broken hydrogen bonds can be reformed. This process helps the material to self-heal, thereby improving the durability and toughness of the material. In addition, the introduction of benzimidazole rings, urea bonds and silicone segments also improves the heat resistance of the coating.
[0014] In the reinforcing filler, ethyl orthosilicate and γ-aminopropyltriethoxysilane are first used as raw materials to coat a layer of silicon dioxide on the surface of alumina to synthesize SiO2@Al2O3 nanomaterials; then glutaraldehyde is used as a cross-linking agent to modify chitosan on the surface of SiO2@Al2O3 nanomaterials to synthesize reinforcing fillers. The reinforcing filler is based on alumina, which is modified for the second time to have excellent dispersibility in the matrix, which can effectively improve the mechanical properties and corrosion resistance of the coating. Among them, the core-shell structure formed by alumina and silica can effectively improve the impact resistance of the coating when the coating is impacted by external force, and reduce the phenomenon of coating cracking caused by external force impact. The introduction of chitosan can synergize with SiO2@Al2O3 nanomaterials to give the coating a certain corrosion resistance. This is due to the coordination bonds formed by chitosan and unpaired electron elements (such as N, O, H, etc.) on the metal surface. These elements or groups can directly form coordination bonds with the empty orbitals on the metal elements, so that the organic molecules are firmly adsorbed on the metal surface to form a protective film, thereby preventing metal corrosion. DETAILED DESCRIPTION
[0015] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0016] Example 1 The modified polyurethane elastomer is prepared by the following steps: Step A1: 0.1 mol of benzimidazole and 100 mL of anhydrous methanol were placed in a reactor, stirred evenly under nitrogen, and then 0.12 mol of vinyltrimethoxysilane was added dropwise while stirring. After the addition was completed, the temperature was raised to 35° C. and reacted for 3 h. After the reaction was completed, rotary evaporation was performed to obtain an intermediate; Step A2: Add 0.05 g of potassium hydroxide to 20 g of ethanol-water solution with a mass ratio of 1:1 and stir evenly, which is recorded as solution 1; under nitrogen conditions, add 4.5 g of dimethyldiethoxysilane, 5.2 g of dimethylethoxysilane, 10.3 g of N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane and 2.4 g of the intermediate into a flask, then add 20 g of solution 1, and increase the system temperature to 55°C, stir and react for 3 hours, then increase the system temperature to 120°C to remove alcohol and water, then collect the product, add 30 g of cyclohexane to the product and stir for 10 minutes, then add 5 g of 732 cation exchange resin and stir for 20 minutes, filter and distill to obtain amino-containing organosilicon; Step A3: Add 0.1 mol polyethylene glycol ( M n =1000) was added into a flask and heated to 120°C for vacuum dehydration for 1h. Argon was introduced, and then the system temperature was lowered to 70°C. 0.15mol of isophorone diisocyanate and 0.001mol of dibutyltin dilaurate were added and reacted for 2h. Then 30mL of toluene, 2g of amino-containing silicone and 3g of ethylenediamine were added and stirred to mix evenly. The mixture was stirred and reacted for 2h. After the reaction was completed, a modified polyurethane elastomer was obtained.
[0017] The reinforcing filler is prepared by the following steps: Step B1: Add 2g of polyvinyl pyrrolidone to 50mL of anhydrous ethanol and disperse evenly, then add 3g of nano-alumina and ultrasonically disperse for 30min, then slowly drop 10mL of the mixed solution, and adjust the pH to 8.5, so that the dropwise addition of the mixed solution is completed within 2h, and then continue to react at 35°C for 4h. After the reaction is completed, centrifuge, wash, and dry to obtain SiO2@Al2O3 nanomaterials. The mixed solution is prepared by mixing ethyl orthosilicate, γ-aminopropyltriethoxysilane, and anhydrous ethanol in a dosage ratio of 0.1g:0.1g:10mL; Step B2: Disperse 5g of chitosan evenly in 10mL of 2wt% sodium hydroxide solution, and refrigerate at -10℃ for 24h. Centrifuge after thawing, and dry the precipitate at 60℃ to obtain pre-treated chitosan. Disperse 1g of pre-treated chitosan in 10mL of deionized water, which is recorded as chitosan solution. Add 1g of SiO2@Al2O3 nanomaterial to 20mL of 2wt% glutaraldehyde solution and disperse evenly. Then increase the system temperature to 45℃ and react for 30min. After the reaction is completed, centrifuge and wash, then add 10mL of chitosan solution, maintain the temperature and continue to react for 2h. After the reaction is completed, centrifuge, wash and dry to obtain reinforced filler.
[0018] Example 2 The modified polyurethane elastomer is prepared by the following steps: Step A1: 0.1 mol of benzimidazole and 100 mL of anhydrous methanol were placed in a reactor, stirred evenly under nitrogen, and then 0.16 mol of vinyltrimethoxysilane was added dropwise while stirring. After the addition was completed, the temperature was raised to 35° C. and reacted for 4 hours. After the reaction was completed, rotary evaporation was performed to obtain an intermediate; Step A2: Add 0.065g potassium hydroxide to 20g ethanol-water solution with a mass ratio of 1:1 and stir evenly, which is recorded as solution 1; under nitrogen conditions, add 4.5g dimethyldiethoxysilane, 7.3g dimethylethoxysilane, 12.2g N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane and 4.8g intermediate into a flask, then add 20g solution 1, and increase the system temperature to 60°C, stir and react for 4h, then increase the system temperature to 125°C to remove alcohol and water, then collect the product, add 30g cyclohexane to the product and stir for 20min, then add 7.5g 732 cation exchange resin and stir for 30min, filter and distill to obtain amino-containing organosilicon; Step A3: Add 0.1 mol polyethylene glycol ( M n =1000) was added into a flask and heated to 130°C for vacuum dehydration for 2h. Argon was introduced, and then the system temperature was lowered to 80°C. 0.2mol of isophorone diisocyanate and 0.003mol of dibutyltin dilaurate were added and reacted for 3h. Then 40mL of toluene, 3g of amino-containing silicone and 4.5g of ethylenediamine were added and stirred to mix evenly. The mixture was stirred and reacted for 2.5h. After the reaction was completed, a modified polyurethane elastomer was obtained.
[0019] The reinforcing filler is prepared by the following steps: Step B1: Add 3g of polyvinyl pyrrolidone to 50mL of anhydrous ethanol and disperse evenly, then add 3g of nano-alumina and ultrasonically disperse for 30min, then slowly drop 10mL of the mixed solution, and adjust the pH to 8.7, so that the dropwise addition of the mixed solution is completed within 2.5h, and then continue to react at 35°C for 4h. After the reaction is completed, centrifuge, wash, and dry to obtain SiO2@Al2O3 nanomaterials. The mixed solution is prepared by mixing ethyl orthosilicate, γ-aminopropyltriethoxysilane, and anhydrous ethanol in a dosage ratio of 0.15g:0.1g:10mL; Step B2: Disperse 5g of chitosan evenly in 10mL of 2.5wt% sodium hydroxide solution, and refrigerate at -10℃ for 24h. Centrifuge after thawing, and dry the precipitate at 60℃ to obtain pre-treated chitosan. Disperse 2g of pre-treated chitosan in 10mL of deionized water, which is recorded as chitosan solution. Add 1g of SiO2@Al2O3 nanomaterial to 25mL of 1.5wt% glutaraldehyde solution and disperse evenly. Then increase the system temperature to 45℃ and react for 30min. After the reaction is completed, centrifuge and wash, then add 10mL of chitosan solution, maintain the temperature and continue to react for 3h. After the reaction is completed, centrifuge, wash and dry to obtain reinforced filler.
[0020] Example 3 The modified polyurethane elastomer is prepared by the following steps: Step A1: 0.1 mol of benzimidazole and 100 mL of anhydrous methanol were placed in a reactor, stirred evenly under nitrogen, and then 0.2 mol of vinyltrimethoxysilane was added dropwise while stirring. After the addition was completed, the temperature was raised to 35° C. and reacted for 5 h. After the reaction was completed, rotary evaporation was performed to obtain an intermediate; Step A2: Add 0.08 g potassium hydroxide to 20 g ethanol-water solution with a mass ratio of 1:1 and stir evenly, which is recorded as solution 1; under nitrogen conditions, add 4.5 g dimethyldiethoxysilane, 10.4 g dimethylethoxysilane, 14.5 g N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane and 7.1 g intermediate into a flask, then add 20 g solution 1, and increase the system temperature to 65°C, stir and react for 5 hours, then increase the system temperature to 130°C to remove alcohol and water, then collect the product, add 30 g cyclohexane to the product and stir for 30 minutes, then add 10 g 732 cation exchange resin and stir for 40 minutes, filter and distill to obtain amino-containing organosilicon; Step A3: Add 0.1 mol polyethylene glycol ( M n=1000) was added into a flask and heated to 140°C for vacuum dehydration for 3 hours. Argon was introduced, and then the system temperature was lowered to 90°C. 0.25 mol of isophorone diisocyanate and 0.005 mol of dibutyltin dilaurate were added and reacted for 4 hours. Then 50 mL of toluene, 4 g of amino-containing silicone and 6 g of ethylenediamine were added and stirred to mix evenly. The mixture was stirred and reacted for 3 hours. After the reaction was completed, a modified polyurethane elastomer was obtained.
[0021] The reinforcing filler is prepared by the following steps: Step B1: 4 g of polyvinyl pyrrolidone was added to 50 mL of anhydrous ethanol and dispersed evenly, and then 3 g of nano-alumina was added and ultrasonically dispersed for 30 min, and then 10 mL of the mixed solution was slowly added dropwise, and the pH was adjusted to 9, so that the addition of the mixed solution was completed within 3 h, and then the reaction was continued at 35 ° C for 4 h. After the reaction was completed, centrifugation, washing, and drying were performed to obtain SiO2@Al2O3 nanomaterials. The mixed solution was prepared by mixing ethyl orthosilicate, γ-aminopropyltriethoxysilane and anhydrous ethanol in a dosage ratio of 0.2 g: 0.1 g: 10 mL; Step B2: Disperse 5g of chitosan evenly in 10mL of 3wt% sodium hydroxide solution, and refrigerate at -10℃ for 24h. Centrifuge after thawing, and dry the precipitate at 60℃ to obtain pre-treated chitosan. Disperse 3g of pre-treated chitosan in 10mL of deionized water, which is recorded as chitosan solution. Add 1g of SiO2@Al2O3 nanomaterial to 30mL of 1wt% glutaraldehyde solution and disperse evenly. Then increase the system temperature to 45℃ and react for 30min. After the reaction is completed, centrifuge and wash, then add 10mL of chitosan solution, maintain the temperature and continue to react for 4h. After the reaction is completed, centrifuge, wash and dry to obtain reinforced filler.
[0022] Example 4 A method for preparing an impact-resistant polyester resin powder coating comprises the following steps: 55 parts of polyester resin (Anhui Shenjian polyester resin 4868), 5 parts of triglycidyl isocyanurate, 7 parts of modified polyurethane elastomer prepared in Example 1, 10 parts of reinforcing filler prepared in Example 1, 1 part of antioxidant BHT, 2 parts of sodium stearate, and 0.5 parts of hydroxymethyl cellulose; The above raw materials are weighed by weight, and each component of the raw materials is mixed and stirred evenly in a stirrer, and then melted, extruded, tableted, crushed, and sieved to obtain a powder with a particle size of 500 meshes to obtain an impact-resistant polyester resin powder coating.
[0023] Example 5 A method for preparing an impact-resistant polyester resin powder coating comprises the following steps: 65 parts of polyester resin (Anhui Shenjian polyester resin 4868), 7 parts of triglycidyl isocyanurate, 8 parts of modified polyurethane elastomer prepared in Example 2, 15 parts of reinforcing filler prepared in Example 2, 2 parts of antioxidant BHT, 2.5 parts of sodium stearate, and 1 part of hydroxymethyl cellulose; The above raw materials are weighed by weight, and each component of the raw materials is mixed and stirred evenly in a stirrer, and then melted, extruded, tableted, crushed, and sieved to obtain a powder with a particle size of 600 meshes to obtain an impact-resistant polyester resin powder coating.
[0024] Example 6 A method for preparing an impact-resistant polyester resin powder coating comprises the following steps: 75 parts of polyester resin (Anhui Shenjian polyester resin 4868), 9 parts of triglycidyl isocyanurate, 10 parts of modified polyurethane elastomer prepared in Example 3, 20 parts of reinforcing filler prepared in Example 3, 3 parts of antioxidant BHT, 3 parts of sodium stearate, and 2 parts of hydroxymethyl cellulose; The above raw materials are weighed by weight, and each component of the raw materials is mixed and stirred evenly in a stirrer, and then melted, extruded, tableted, crushed, and sieved to obtain a powder with a particle size of 600 meshes to obtain an impact-resistant polyester resin powder coating.
[0025] Comparative Example 1 This comparative example is a polyester resin powder coating, which differs from Example 6 in that a commercially available polyurethane elastomer is used instead of the modified polyurethane elastomer prepared in Example 3, and the rest are the same.
[0026] Comparative Example 2 This comparative example is a polyester resin powder coating, which differs from Example 6 in that nano-alumina is used instead of the reinforcing filler prepared in Example 3, and the rest are the same.
[0027] The polyester resin powder coatings prepared in Examples 4-6 and Comparative Examples 1-2 were sprayed onto a 1.0 mm thick tinplate by electrostatic spraying, the curing conditions were 200°C / 10min, the coating film thickness was controlled to be 60-90 μm, and finally the test sample was placed at 25°C for 24 hours before the performance test was performed: Impact resistance test: tested according to GB / T 1732-2020 standard; Heat resistance test: Place the coating in an oven at 300°C for 48 hours and observe the changes on the coating surface; Corrosion resistance test: Tested in accordance with GB / T 10125-2021 standard; The test results are shown in the following table:
[0028] It can be seen from the above table that the polyester resin powder coating prepared by the present invention has an impact strength of 50kg / cm2-55kg / cm2 after the impact resistance test, indicating that the coating has good impact resistance; the heat resistance test found that there is no obvious change on the coating surface, and the coating has good heat resistance; the corrosion resistance test found that there is no obvious corrosion on the coating surface, and the coating has good corrosion resistance.
[0029] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.
Claims
1. An impact-resistant polyester resin powder coating, It is characterized in that The invention comprises the following raw materials in parts by weight: 55-75 parts of polyester resin, 5-9 parts of curing agent, 7-10 parts of modified polyurethane elastomer, 10-20 parts of reinforcing filler, 1-3 parts of antioxidant, 2-3 parts of dispersant and 0.5-2 parts of leveling agent; The modified polyurethane elastomer is prepared by the following steps: Step A1: benzimidazole, anhydrous ethanol and vinyltrimethoxysilane are mixed, nitrogen is introduced, reacted, and rotary evaporated to obtain an intermediate; Step A2: Under nitrogen, dimethyldiethoxysilane, dimethylethoxysilane, N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane, the intermediate and solution 1 are mixed for reaction, the product is collected, cyclohexane and 732 cation exchange resin are added in sequence, stirred, filtered and distilled to obtain amino-containing organosilicon; Step A3: After dehydrating the polyethylene glycol in vacuo, argon is introduced, isophorone diisocyanate and dibutyltin dilaurate are added to react, and then toluene, amino-containing silicone and ethylenediamine are added to react to obtain a modified polyurethane elastomer.
2. The impact-resistant polyester resin powder coating according to claim 1, It is characterized in that In step A1, the dosage ratio of benzimidazole, vinyltrimethoxysilane and anhydrous methanol is 0.1 mol: 0.12-0.2 mol: 100 mL, the reaction temperature in step A1 is 35° C., and the reaction time is 3-5 h.
3. The impact-resistant polyester resin powder coating according to claim 1, It is characterized in that In step A2, the mass ratio of dimethyldiethoxysilane, dimethylethoxysilane, N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane, intermediate, solution 1, cyclohexane and 732 cation exchange resin is 4.5: 5.2-10.4: 10.3-14.5: 2.4-7.1: 20: 30: 5-10. During the mixed reaction in step A2, the temperature is first raised to 55-65° C. for reaction for 3-5 hours, and then raised to 120-130° C. to remove alcohol and water. The stirring time after the addition of cyclohexane and 732 cation exchange resin is 10-30 minutes and 20-40 minutes, respectively.
4. The impact-resistant polyester resin powder coating according to claim 1, It is characterized in that In step A2, solution 1 is prepared by mixing potassium hydroxide, ethanol and deionized water in a mass ratio of 0.05-0.08:10:
10.
5. The impact-resistant polyester resin powder coating according to claim 1, It is characterized in that In step A3, the dosage ratio of polyethylene glycol, isophorone diisocyanate, dibutyltin dilaurate, toluene, amino-containing silicone and ethylenediamine is 0.1 mol: 0.15-0.25 mol: 0.001-0.005 mol: 30-50 mL: 2-4 g: 3-6 g, the dehydration temperature of polyethylene glycol is 120-140 ° C, the time is 1-3 h, the reaction temperature of the elastomer is 70-90 ° C, and the two reaction times are 2-4 h and 2-3 h respectively.
6. The impact-resistant polyester resin powder coating according to claim 1, It is characterized in that The reinforcing filler is prepared by the following steps: Step B1: Add polyvinyl pyrrolidone to anhydrous ethanol and disperse it evenly, then add nano-alumina and ultrasonically disperse it for 30 minutes, slowly drop the mixture, and adjust the pH to 8.5-9. The mixture is added dropwise within 2-3 hours, and then the reaction is continued at 35°C for 4 hours. After the reaction is completed, centrifuge, wash and dry to obtain SiO 2 @Al 2 O 3 Nanomaterials; Step B2: Disperse 1-3 g of pre-treated chitosan in 10 mL of deionized water, referred to as chitosan solution; 2 @Al 2 O 3 The nanomaterial is evenly dispersed in a 1wt%-2wt% glutaraldehyde solution, and then the system temperature is raised to 45°C for reaction for 30 minutes. After the reaction is completed, centrifuge and wash, and then add chitosan solution, maintain the temperature and continue to react for 2-4 hours. After the reaction is completed, centrifuge, wash and dry to obtain a reinforced filler.
7. The impact-resistant polyester resin powder coating according to claim 6, It is characterized in that In step B1, the dosage ratio of polyvinyl pyrrolidone, anhydrous ethanol, nano-alumina and the mixed solution is 2-4g:50mL:3g:10mL, and the mixed solution is prepared by mixing ethyl orthosilicate, γ-aminopropyltriethoxysilane and anhydrous ethanol in a dosage ratio of 0.1-0.2g:0.1g:10mL.
8. The impact-resistant polyester resin powder coating according to claim 6, It is characterized in that Step B2 SiO 2 @Al 2 O 3 The dosage ratio of the nano material, glutaraldehyde solution and chitosan solution is 1g:20-30mL:10mL.
9. An impact-resistant polyester resin powder coating according to claim 6, It is characterized in that In step B2, the pretreated chitosan is prepared by the following steps: 5 g of chitosan is evenly dispersed in 10 mL of 2wt%-3wt% sodium hydroxide solution, and refrigerated at -10°C for 24 hours, centrifuged after thawing, and the precipitate is dried at 60°C to obtain the pretreated chitosan.
10. A method for preparing an impact-resistant polyester resin powder coating according to any one of claims 1 to 9, It is characterized in that The following steps are involved: The raw materials are weighed by weight, and each component of the raw materials is mixed and stirred evenly in a stirrer, and then melted, extruded, tableted, crushed, and sieved to obtain a powder with a particle size of 500-600 meshes to obtain an impact-resistant polyester resin powder coating.
Citation Information
Patent Citations
Organic silicon static-conducting coating based on silicon-based imidazolium ionic liquid
CN109355009A
Preparation method of high-bonding high-heat dissipation paint
CN110016286A
Low-temperature-resistant and impact-resistant polyurethane elastomer and processing technology thereof
CN115873199A
Weather-resistant powder coating, coating and preparation method
CN116102908A
Weather-resistant powder coating and preparation method thereof
CN118185434A
Cited By
Fixing line for carton reinforcement and preparation method thereof
CN119241993A
Polyester film with high adhesion fastness to UV (ultraviolet) material and preparation method of polyester film
CN119261338A