Thermally-induced dimming coating liquid and externally-attached glass film on car roof
By using a thermodynamic dimming coating solution in the glass film on the roof, using a combination of hydrazide chain extender and ionic liquid, the coating that automatically adjusts transparency according to photothermal conditions is achieved, and the existing vehicles are solved The problem of poor thermal insulation effect of glass film on the top has enhanced thermal insulation and privacy protection, and provided self-repair and aesthetic functions.
Patent Information
- Application Number
- CN202411374852.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-22
AI Technical Summary
The existing roof glass film is easily saturated after absorbing heat from sunlight, resulting in a reduced thermal insulation effect and unable to effectively block the increase in the temperature in the car.
Using a thermogenic dimming coating liquid, by introducing hydrazide chain extenders and ionic liquids into the polyurethane, the cured coating can automatically adjust the transparency according to the external photothermal conditions, thereby adjusting the light transmittance and reducing the sun. The radiant energy of light enters the car.
It realizes the function of automatically adjusting the light transmittance according to the external ambient temperature, enhances the heat insulation effect, and has self-repair performance, reduces the increase in the temperature in the car, and provides privacy protection and beautiful personalized appearance.
Smart Images

Figure CN118995029A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a coating liquid, in particular to a thermoluminescent coating liquid. The invention also provides a roof external glass film. Background Art
[0002] Compared with traditional small car sunroofs, full glass roofs and panoramic sunroofs have won wide acclaim for their excellent transparency and high light transmittance. They not only make the interior space appear more spacious, but also allow passengers to enjoy the boundless sky when they look up. Drivers can also enjoy the wonderful scenery of light and shadow, which adds a lot of romance and pleasure, so they are very popular among consumers. However, everything has its two sides. While large panoramic sunroofs and full glass roofs improve the driving experience, they also bring some problems that are difficult to ignore, such as poor sun protection and fragility. Especially in the hot summer, the strong sunlight directly hits the roof. Even if the air conditioner in the car is adjusted to the lowest temperature, the large area of glass above the head is still like a hot oven, which is a headache.
[0003] In order to solve this problem, roof glass film products came into being. Roof glass films are divided into external films and internal films. Internal glass films are made of PET material and are attached to the inside of the roof glass. They generally provide sun protection and heat insulation through reflection, and can effectively block ultraviolet rays and part of the heat, reducing the damage to items and people in the car caused by ultraviolet radiation. In addition, enhancing safety is also an important feature of roof glass films, so external glass films came into being. External glass films are made of TPU material, which can effectively reduce the impact of the outside world on the roof glass, greatly reducing the possibility of the roof glass being smashed, so external glass films are becoming more and more popular with customers.
[0004] At present, the glass film on the roof mainly achieves the heat insulation effect by absorbing the heat from the sun, and this purpose is achieved by adding some heat-absorbing inorganic materials. However, this kind of glass film on the roof will reach a saturation state after absorbing a certain amount of heat and can no longer absorb heat. Over time, the saturation of heat absorption will gradually decrease, causing heat to be transferred into the car, causing the temperature inside the car to rise, affecting the heat insulation effect.
[0005] Therefore, the applicant proposed the present invention. Summary of the invention
[0006] An object of the present invention is to provide a thermoluminescent coating solution, the coating obtained by curing the coating solution can automatically adjust its light transmittance according to external light and heat conditions.
[0007] Another object of the present invention is to provide a roof glass film that can automatically adjust its light transmittance according to the light and heat conditions of the external environment.
[0008] In order to achieve the above first object of the invention, the present invention provides a thermoluminescent coating liquid, which includes the following components and their weight parts: Modified polyol resin 400~600 Isocyanate curing agent 50~200 Hydrazide chain extender 23~80 Catalyst 5~25 Ionic liquid 95~350 UV absorber 5~18 Organic solvents: 900-2000.
[0009] The modified polyol resin is a resin containing two or more hydroxyl groups, and is preferably at least one of a polycarbonate polyol resin and a polycaprolactone polyol resin.
[0010] When the modified polyol resin is a polycarbonate polyol resin, it is further preferably selected from at least one of Covestro's C1100, C1200, C2200, C3100XP, and CXP2716.
[0011] When the modified polyol resin is a polycaprolactone polyol resin, it is further preferably selected from at least one of PCL210N, PCL220N, PCL210CP, PCL230N and PCL205H produced by Daicel Corporation of Japan.
[0012] The isocyanate curing agent is preferably a trimer of diisocyanate, and is further preferably at least one of toluene diisocyanate (TDI) trimer, diphenylmethane diisocyanate (MDI) trimer, hexamethylene diisocyanate (HDI) trimer, and isophorone diisocyanate (IPDI) trimer.
[0013] The hydrazide chain extender is preferably selected from at least one of malonic dihydrazide, succinic acid dihydrazide, adipic acid dihydrazide and sebacic acid dihydrazide.
[0014] The catalyst is preferably selected from the group consisting of dibutyltin dilaurate, stannous isooctanoate, zinc isooctanoate, and bismuth isooctanoate.
[0015] The ionic liquid is preferably at least one of 1-butyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide and 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.
[0016] The ultraviolet absorber is preferably at least one of TINUVIN 99-2, TINUVIN 384-2, TINUVIN 400, TINUVIN477, TINUVIN 900, and TINUVIN1130.
[0017] The organic solvent is preferably selected from at least one of esters, ketones and aromatic hydrocarbons.
[0018] Furthermore, the present invention provides a thermoluminescent coating solution, which also includes the following components and their weight parts: Light stabilizer 5~18.
[0019] Furthermore, the light stabilizer is preferably at least one of TINUVIN 123, TINUVIN 144, TINUVIN 152, TINUVIN 249, and TINUVIN 292.
[0020] The invention discloses a thermoluminescent coating liquid. By introducing hydrazide groups and ionic liquids into polyurethane, the coating obtained by curing has an obvious thermoluminescent effect, that is, it can automatically adjust its light transmittance according to the light and heat conditions of the external environment.
[0021] The specific mechanism is as follows: when hydrazide chain extenders are introduced into polyurethane, hydrazide groups react with isocyanate to form acylaminourea. These groups can provide more hydrogen bond acceptors and donors. On the one hand, more hydrogen bonds can be formed between polyurethane chain segments, thereby enhancing the mechanical strength and self-healing properties of the coating obtained by polyurethane curing. On the other hand, these hydrogen bond acceptors can be paired with hydrogen bond donors of ionic liquids to form hydrogen bonds between ionic liquids and polyurethanes at room temperature. Ionic liquids can be well dispersed in polyurethanes and have good compatibility. At this time, the coating obtained by polyurethane curing is transparent. However, as the external environment temperature increases, the hydrogen bonds between the ionic liquid and the polyurethane will break, and the ionic liquid will precipitate from the polyurethane. At this time, the coating changes from a transparent state to a frosted state (opaque state). As the temperature drops again, hydrogen bonds are re-formed between the ionic liquid and the polyurethane. At this time, the coating changes from a frosted state to a transparent state (reversible change).
[0022] In order to achieve the above second invention objective, the present invention provides a roof glass film, comprising a thermo-modulated light-adjusting layer obtained by curing the aforementioned mid-coating liquid, a TPU substrate layer, a pressure-sensitive adhesive layer and a release film layer, which are compounded in sequence.
[0023] The thickness of the thermotropic dimming layer is preferably 6 μm to 12 μm.
[0024] The material of the TPU substrate layer is preferably aliphatic TPU, the surface hardness is preferably 80A-93A, the visible light transmittance is preferably above 90%, the elongation at break is preferably above 300%, the haze is preferably below 2%, and the thickness is preferably 100μm-300μm.
[0025] The material of the pressure-sensitive adhesive layer is preferably transparent acrylic pressure-sensitive adhesive or polyurethane pressure-sensitive adhesive, the visible light transmittance is preferably above 90%, and the thickness is preferably 20 μm to 50 μm.
[0026] The release film layer is preferably a PET release film, and more preferably a white PET release film, the haze is preferably above 70%, the release force is preferably within 20 g / inch, and the thickness is preferably 50 μm to 100 μm.
[0027] Furthermore, the layered structure of the roof glass film provided by the present invention further includes a protective film layer, and the protective film layer is compounded to the surface of the thermoluminescent layer on the side away from the TPU substrate layer.
[0028] The material of the protective film layer is preferably transparent PET, and is further preferably a PET protective film with silicone or a PET release film, and the thickness is preferably 23 μm to 75 μm.
[0029] The glass film for attaching the roof to the outside of the vehicle can be prepared by first coating a pressure-sensitive adhesive layer and then coating a thermo-optical dimming coating liquid, and the coating method is preferably roller coating, slit coating or comma blade coating.
[0030] The present invention also provides a method for preparing a glass film for a roof, and the specific steps are as follows: Step 1, pre-prepare the thermo-optical dimming coating liquid according to the proportion; Step 2: coating the pressure-sensitive adhesive liquid on the release film layer, drying at 80-120° C. for 2-3 min to form a pressure-sensitive adhesive layer with a thickness of 20 μm-50 μm, and then compounding with a TPU substrate layer with a thickness of 100 μm-300 μm; Step 3: coating the reverse side of the TPU substrate layer in the above step 2 with a thermo-optical dimming coating liquid, curing under the conditions of 80-140° C. for 2-4 min to form a thermo-optical dimming layer with a thickness of 6 μm-12 μm, and then compounding a protective film layer with a thickness of 23 μm-75 μm on the surface; Step 4: Ripening the semi-finished product in step 3 at 40-60° C. for 24-72 hours to obtain a finished product.
[0031] Compared with the prior art, the thermoluminescent coating liquid and the roof glass film obtained by the present invention have the following technical effects: 1) The present invention provides a thermoluminescent coating liquid, the coating obtained by curing can automatically adjust its light transmittance according to external light and heat conditions.
[0032] 2) The thermoluminescent coating liquid provided by the present invention has a coating obtained by curing and has good repairability, and small scratches on the surface can be repaired at high temperature.
[0033] 3) The present invention provides a roof glass film that not only has functions such as blocking ultraviolet rays and repairing scratches, but also has a thermo-induced dimming function, that is, it can adjust its own light transmittance according to the external environment temperature. At room temperature (generally below 30°C), the roof glass film is transparent. As the temperature rises, the light transmittance of the roof glass film decreases, and it changes from a transparent state to a frosted state, thereby reducing the radiation energy entering the sun. It can be seen that the present invention blocks radiant heat by reducing the visible light transmittance, thereby effectively solving the technical problem that "the existing roof glass film that achieves heat insulation by absorbing heat from sunlight is prone to poor heat insulation effect".
[0034] 4) The roof glass film provided by the present invention can also protect privacy. When the roof glass film is in a frosted state, it can reduce the outside world's prying into the situation inside the car, thereby increasing the privacy of the interior space of the car. In terms of aesthetics, the roof glass film can change the color of the car body, adding a personalized and beautiful appearance to the vehicle.
[0035] 5) The roof glass film provided by the present invention has a simple layered structure, obvious heat insulation effect, and broad application prospects. It can be applied not only to roof glass, but also to architectural glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic diagram of the layered structure of a glass film applied to the exterior of a vehicle roof.
[0037] In the figure: white PET release film 1, pressure-sensitive adhesive layer 2, TPU substrate 3, thermo-induced dimming layer 4, PET protective film 5. DETAILED DESCRIPTION
[0038] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention. Embodiment 1:
[0039] As an embodiment of the present invention, a thermoluminescent coating liquid provided in this embodiment includes the following components and their weight parts: 400 parts of modified polyol resin (C3100XP, Covestro), 135 parts of isocyanate curing agent (hexamethylene diisocyanate, Aladdin reagent), 53 parts of hydrazide chain extender (malonic acid hydrazide, Aladdin reagent), 6 parts of catalyst (stannous isooctanoate, Aladdin reagent), 120 parts of ionic liquid (1-butyl-2,3-dimethylimidazole bis(trifluoromethanesulfonyl)imide salt, Aladdin reagent), 9 parts of ultraviolet absorber (TINUVIN 400, BASF), 9 parts of light stabilizer (TINUVIN 123, BASF), and 1,100 parts of organic solvent (toluene).
[0040] The specific preparation process of the above-mentioned thermoluminescent coating liquid is as follows: According to the above weight ratio, a modified polyol resin (C3100XP, Covestro), a hydrazide chain extender (malonic acid hydrazide, Aladdin reagent), a catalyst (stannous isooctanoate, Aladdin reagent), an ionic liquid (1-butyl-2,3-dimethylimidazole bis(trifluoromethanesulfonyl)imide salt, Aladdin reagent), a UV absorber (TINUVIN 400, BASF), a light stabilizer (TINUVIN 123, BASF) and an organic solvent (toluene) were added into a container and stirred at high speed for 30 minutes until the mixture was uniformly stirred.
[0041] Before coating, add isocyanate curing agent (hexamethylene diisocyanate, Aladdin reagent), and stir at high speed for 30 minutes until it is evenly stirred for use.
[0042] In addition, this embodiment provides a roof glass film, the layered structure of which is as follows: Figure 1 As shown, the specific preparation process is as follows: Step 1: Apply a pressure-sensitive adhesive liquid (Henkel, Loctite 8087) on one side of a 50 μm thick white PET release film (Toray, XZ31SR), dry at 110°C for 2 min to form a pressure-sensitive adhesive layer with a dry adhesive thickness of 20 μm, and then cover the pressure-sensitive adhesive layer on one side of a 100 μm thick TPU substrate (49510, Argotec).
[0043] Step 2: coating the aforementioned thermo-optical dimming coating liquid on the other side of the TPU substrate in step 1, curing conditions: 120° C., 3 min, the thickness of the thermo-optical dimming layer after drying is 6 μm, and finally covering the surface of the thermo-optical dimming layer with a 23 μm PET protective film (Yihua Dongli, G01); Step three, placing the semi-finished product in step two into a 50°C curing chamber, after 72 hours, a roof glass film with thermo-induced dimming and self-repairing effects can be obtained. Embodiment 2:
[0044] As a second embodiment of the present invention, a thermoluminescent coating liquid provided in this embodiment includes the following components and their weight parts: 500 parts of modified polyol resin (PCL220N, Daicel), 76 parts of isocyanate curing agent (hexamethylene diisocyanate, Aladdin reagent), 29 parts of hydrazide chain extender (succinic acid dihydrazide, Aladdin reagent), 12 parts of catalyst (stannous isooctanoate, Aladdin reagent), 180 parts of ionic liquid (1-butyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt, Aladdin reagent), 10 parts of ultraviolet absorber (TINUVIN 400, BASF), 10 parts of light stabilizer (TINUVIN 123, BASF), and 1200 parts of organic solvent (toluene).
[0045] The preparation method of the thermoluminescent coating liquid provided in this embodiment is consistent with that of the aforementioned embodiment 1.
[0046] Similarly, this embodiment also provides a roof glass film, whose layered structure is consistent with that of the aforementioned embodiment 1, but the specific preparation process is as follows: Step 1: Apply a pressure-sensitive adhesive liquid (Henkel, Loctite 8087) on one side of a 75 μm thick white PET release film (Toray, XZ31SR), dry at 110°C for 2 min to form a pressure-sensitive adhesive layer with a dry adhesive thickness of 35 μm, and then cover the pressure-sensitive adhesive layer on one side of a 200 μm thick TPU substrate (49510, Argotec).
[0047] Step 2: coating the aforementioned thermo-optical dimming coating liquid on the other side of the TPU substrate in step 1, curing conditions: 120° C., 3 min, the thickness of the thermo-optical dimming layer after drying is 9 μm, and finally covering the surface of the thermo-optical dimming layer with a 50 μm PET protective film (Yihua Dongli, G01); Step three, placing the semi-finished product in step two into a 50°C curing chamber, after 72 hours, a roof glass film with thermo-induced dimming and self-repairing effects can be obtained. Embodiment 3:
[0048] As a third embodiment of the present invention, a thermoluminescent coating liquid provided in this embodiment includes the following components and their weight parts: 600 parts of modified polyol resin (PCL230N, Daicel), 70 parts of isocyanate curing agent (toluene diisocyanate, Aladdin reagent), 46 parts of hydrazide chain extender (sebacic acid hydrazide, Aladdin reagent), 22 parts of catalyst (stannous isooctanoate, Aladdin reagent), 286 parts of ionic liquid (1-butyl-3-methylimidazole bis (trifluoromethanesulfonyl) imide salt, Aladdin reagent), 11 parts of ultraviolet absorber (TINUVIN 400, BASF), 11 parts of light stabilizer (TINUVIN 123, BASF), and 1570 parts of organic solvent (toluene).
[0049] The preparation method of the thermoluminescent coating liquid provided in this embodiment is also consistent with the above-mentioned embodiment 1.
[0050] In addition, this embodiment also provides a roof glass film, whose layered structure is consistent with the aforementioned embodiment 1, but the specific preparation process is as follows: Step 1: Apply a pressure-sensitive adhesive liquid (Henkel, Loctite 8087) on one side of a 100 μm thick white PET release film (Toray, XZ31SR), dry at 110°C for 2 min to form a pressure-sensitive adhesive layer with a dry adhesive thickness of 50 μm, and then cover the pressure-sensitive adhesive layer on one side of a 300 μm thick TPU substrate (49510, Argotec).
[0051] Step 2: The thermo-optical dimming coating liquid is coated on the other side of the TPU substrate in step 1, and the curing condition is 120° C. for 3 min. After drying, the thickness of the thermo-optical dimming layer is 12 μm. Finally, a 75 μm PET protective film (Yihua Dongli, G01) is covered on the surface of the thermo-optical dimming layer. Step three, placing the semi-finished product in step two into a 50°C curing chamber, after 72 hours, a roof glass film with thermo-induced dimming and self-repairing effects can be obtained.
[0052] Comparative Example 1: This comparative example provides a method for preparing a self-repairing coating liquid, and the specific preparation process is as follows: Add 400 parts of modified polyol resin (C3100XP, Covestro), 5 parts of catalyst (stannous isooctanoate, Aladdin reagent), 7 parts of ultraviolet absorber (TINUVIN 400, BASF), 7 parts of light stabilizer (TINUVIN 123, BASF) and 730 parts of toluene into a container and stir at high speed for 30 minutes until the mixture is uniformly stirred.
[0053] Before coating, add 68 parts of isocyanate curing agent (hexamethylene diisocyanate, Aladdin reagent) and stir at high speed for 30 minutes until it is evenly stirred for use.
[0054] Similarly, this comparative example provides a roof glass film, and the specific preparation process is as follows: Step 1: Apply a pressure-sensitive adhesive liquid (Henkel, Loctite 8087) on one side of a 50 μm thick white PET release film (Toray, XZ31SR), dry at 110°C for 2 min to form a pressure-sensitive adhesive layer with a dry adhesive thickness of 20 μm, and then cover the pressure-sensitive adhesive layer on one side of a 100 μm thick TPU substrate (49510, Argotec).
[0055] Step 2: The self-repairing coating liquid is coated on the other side of the TPU substrate in step 1, and the curing condition is 120°C for 3 minutes. After drying, the thickness of the self-repairing layer is 6 μm. Finally, a 23 μm PET protective film (Yihua Dongli, G01) is covered on the surface of the self-repairing layer. Step three, put the semi-finished product in step two into a 50°C curing chamber. After 72 hours, a roof glass film with self-repairing effect can be obtained.
[0056] Comparative Example 2: This comparative example provides another method for preparing a self-repairing coating liquid, and the specific preparation process is as follows: Add 600 parts of modified polyol resin (PCL230N, Daicel), 19 parts of catalyst (stannous isooctanoate, Aladdin reagent), 10 parts of ultraviolet absorber (TINUVIN 400, BASF), 10 parts of light stabilizer (TINUVIN 123, BASF) and 1000 parts of toluene into a container and stir at high speed for 30 minutes until the mixture is uniformly stirred.
[0057] Before coating, add 35 parts of isocyanate curing agent (hexamethylene diisocyanate, Aladdin reagent) and stir at high speed for 30 minutes until it is evenly stirred for use.
[0058] In addition, this comparative example provides another type of roof glass film, and the specific preparation process is as follows: Step 1: Apply a pressure-sensitive adhesive liquid (Henkel, Loctite 8087) on one side of a 100 μm thick white PET release film (Toray, XZ31SR), dry at 110°C for 2 min to form a pressure-sensitive adhesive layer with a dry adhesive thickness of 50 μm, and then cover the pressure-sensitive adhesive layer on one side of a 300 μm thick TPU substrate (49510, Argotec).
[0059] Step 2: The self-repairing coating liquid is coated on the other side of the TPU substrate in step 1, and the curing condition is 120° C. for 3 min. The thickness of the self-repairing coating after drying is 12 μm. Finally, a 75 μm PET protective film (Yihua Dongli, G01) is covered on the surface of the self-repairing coating. Step three, put the semi-finished product in step two into a 50°C curing chamber. After 72 hours, a roof glass film with self-repairing effect can be obtained.
[0060] VLT(20℃) VLT(35℃) VLT(50℃) Restorative Example 1 90.7% 19.8% 10.2% qualified Example 2 90.6% 11.0% 9.5% qualified Example 3 90.3% 8.8% 8.5% qualified Comparative Example 1 90.8% 90.7% 90.4% qualified Comparative Example 2 90.2% 90.4% 90.4% qualified From the above test data, it can be known that the visible light transmittance (VLT) of the roof glass film provided by the present invention will gradually decrease with the increase of temperature, so it has a thermo-induced dimming effect, can block the entry of heat, and it still has good repairability, and tiny scratches on the surface can be repaired at high temperature.
[0061] The test methods for each performance in the above table are as follows: 1. Visible light transmittance (VLT) Select a piece of glass film for the roof, remove the release film and protective film, stick it on a 3mm transparent glass, use a UV-visible spectrophotometer (Agilent Cary5000) to test the transmittance in the 380-780nm band, and then calculate the visible light transmittance according to GB / T2680.
[0062] 2. Self-healing test Select a piece of glass film for the roof, remove the release film and protective film, wet-apply it on a black paint panel, and slide 500g of #0000 steel wool back and forth on the surface of the glass film three times to observe whether the surface scratches can be restored within half an hour at 60 degrees Celsius. If they can be restored, they are considered qualified.
[0063] The present invention is not limited to the above-mentioned optimal implementation mode. Anyone can derive other various forms of products under the inspiration of the present invention. However, no matter what changes are made in the shape or structure, all technical solutions that are the same or similar to those of the present application fall within the protection scope of the present invention.
Claims
1. A thermoluminescent coating liquid, Its characteristics are The components of the coating solution and their weight parts are: Modified polyol resin 400~600 Isocyanate curing agent 50~200 Hydrazide chain extender 23~80 Catalyst 5~25 Ionic liquid 95~350 UV absorber 5~18 Organic solvents 900-2000; Wherein, the modified polyol resin is a resin containing two or more hydroxyl groups.
2. The thermoluminescent coating liquid according to claim 1, Its characteristics are The components of the coating solution and their weight parts also include: Light stabilizer 5~18.
3. The thermoluminescent coating liquid according to claim 1, Features: The modified polyol resin is at least one of a polycarbonate polyol resin and a polycaprolactone polyol resin.
4. The thermoluminescent coating liquid according to claim 1, Features: The isocyanate curing agent is a trimer of diisocyanate.
5. The thermoluminescent coating liquid according to claim 1, Features: The hydrazide chain extender is at least one of malonic dihydrazide, succinic acid dihydrazide, adipic acid dihydrazide and sebacic acid dihydrazide.
6. The thermoluminescent coating liquid according to claim 1, Features: The catalyst is one of dibutyltin dilaurate, stannous isooctanoate, zinc isooctanoate and bismuth isooctanoate.
7. The thermoluminescent coating liquid according to claim 1, Features: The ionic liquid is at least one of 1-butyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide and 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.
8. A roof glass film, comprising a TPU substrate layer, a pressure-sensitive adhesive layer and a release film layer, Its characteristics are Also includes: The thermoluminescent layer obtained by curing the coating liquid according to any one of claims 1 to 7, wherein the thermoluminescent layer, the TPU substrate layer, the pressure-sensitive adhesive layer and the release film layer are compounded in sequence.
9. The roof glass film according to claim 8, Its characteristics are It also includes: a protective film layer, which is compounded to a surface of the thermoluminescent layer on one side away from the TPU substrate layer.
Citation Information
Patent Citations
Window film with automatically adjustable light transmittance
CN103481564A
Self-repairing and oil stain-preventing coating and preparation method thereof, and protective film containing same and preparation method thereof
CN108084861A
Self-repairing scratch-resistant polyurethane coating and preparation method thereof
CN113088176A
Self-cleaning and self-repairing coating coating liquid of vehicle paint protective film and vehicle paint protective film
CN115232547A