Preparation method of dual-curing adhesive layer and mobile phone protective film thereof
Through the preparation method of the double curing adhesive layer, combined with supercritical treatment and vacuum defoaming technology, a five-layer structure mobile phone protective film suitable for curved screen was prepared, which solved the problems of short service life and difficulty in attaching the existing protective film, and realized the Better fit and fingerprint unlocking accuracy.
Patent Information
- Application Number
- CN202310574309.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
AI Technical Summary
The existing mobile phone screen protector has a short service life on curved screens and mobile phones, and the traditional protective film is difficult to adhere to, which cannot meet the needs of modern living environments.
Using the preparation method of the double curing adhesive layer, a five-layer mobile phone protective film, including PET release layer, is prepared by configuring modified polyurethane acrylate, special functional agglomerated polyurethane acrylate and other raw materials, combined with supercritical treatment and vacuum defoaming technology. , self-healing coating, double curing adhesive layer and pressure-sensitive adhesive layer to adapt to the shape of the curved screen and enhance the fit through UV lamp curing.
It improves the service life and fit of the mobile phone screen protector, meets the needs of curved screens, and does not require a base film, avoids fingerprint unlocking deviation caused by optical degree differences, and ensures the accuracy of fingerprint unlocking under-screen.
Smart Images

Figure HDA0004239486520000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mobile phone screen protective films, and in particular to a preparation method of a double-cured adhesive layer and a mobile phone protective film thereof. Background Art
[0002] With the rapid development of electronic technology, various electronic products are constantly being innovated, and curved screen mobile phones have been promoted more widely due to their better user experience. As major mobile phone manufacturers have launched full-screen mobile phones, the screen-to-body ratio is getting higher and higher. Full-screen mobile phones have become the current development trend of mobile phone screens. Nowadays, the edges and screens of many mobile phones are designed into curved structures, such as curved screen mobile phones. The screen protective films currently on the market generally use a single layer of film, which is not very hard and is easily scratched by friction or relatively large impact. The overall structural curing strength is poor, resulting in a short service life. Obviously, it cannot meet the requirements of our current living environment.
[0003] In addition, in order to prevent the screen surface of their beloved mobile phone from being scratched or worn by hard objects and extend its service life, consumers will choose to stick a protective film on the mobile phone screen. However, the curved screen is different from the flat screen. The curved edge will make it difficult to stick the traditional protective film on the mobile phone screen. The post-cured protective film solves this problem better. Summary of the invention
[0004] The present invention aims to provide a method for preparing a dual-curing adhesive layer and a mobile phone protective film thereof. The raw materials do not contain a difficult-to-degrade polymer plastic film. Related process improvements enable the film to better fit the curved mobile phone screen, thereby protecting the mobile phone screen and providing a better user experience.
[0005] The specific implementation scheme of the preparation method of a dual-curing adhesive layer and a mobile phone protective film thereof according to the present invention is as follows:
[0006] S1, configure the dual-curing adhesive layer raw materials according to the mass ratio
[0007] Prepare the raw materials according to the mass ratio: modified polyurethane acrylate: 20 parts, special functional group polyurethane acrylate: 20-30 parts, isobornyl acrylate: 10-20 parts, cycloaliphatic acrylate: 10-20 parts, 4-hydroxybutyl acrylate: 10-20 parts, diisocyanate-terminated polyester polyol curing agent: 1-5 parts, 1-hydroxycyclohexyl phenyl ketone: 2-3 parts, diphenyl-(2,4,6-trivalent benzoyl)phosphine oxide: 2-3 parts;
[0008] S2, dual-cured adhesive layer obtained by supercritical treatment
[0009] The mixed solution is placed in a vacuum degassing device for vacuum degassing to obtain a pre-solution, the vacuum degree is 0.1-0.5Pa, and the pressure holding time is 20-40min;
[0010] The pre-solution is subjected to supercritical treatment to obtain a dual-cured adhesive layer at a treatment temperature of 100°C-130°C, a pressure of 20-30MPa, and a time of 2-4h. The pore density of the dual-cured adhesive layer is 10 12 -10 15 / cm 3 , the light transmittance of the dual-curing adhesive layer is greater than 90%, the haze is less than 2%, and the thickness range is 0.08-0.12mm;
[0011] S3, stacking according to the designed structure to obtain a mobile phone protective film
[0012] From top to bottom: PET release layer, self-healing coating, dual-curing adhesive layer, pressure-sensitive adhesive layer, PET release layer;
[0013] Furthermore, the upper PET release layer and the lower PET release layer are both release films, the thickness of the release films is 40-60um, and the light transmittance is greater than 88%;
[0014] Furthermore, the release film is obtained by mixing raw materials, the mixing method is vacuum ball milling + vacuum degassing treatment, the ball milling speed is 100-200rpm, and TEMOPO modified nanocellulose is added to the raw materials before ball milling, the cellulose length is 200-600nm, and the diameter is 3-10nm;
[0015] Furthermore, the self-repairing coating is one of a polyurethane elastic coating or a UV elastic self-repairing coating, the self-repairing coating is modified by a silane coupling agent KH550, the material has an adhesive strength of 0.7-1.1 MPa, and a thermal weight loss temperature of 230-270°C;
[0016] Furthermore, the self-repairing coating is coated on the double-cured adhesive layer by a coating process, the thickness of the self-repairing coating is 15-20um, the coating process refers to ultrasonic thermal coating, the ultrasonic frequency is 0.5-0.8KHz, the coating temperature is 60-100°C, and the processing time is 10-30min;
[0017] Furthermore, the pressure-sensitive adhesive layer is one of polyurethane pressure-sensitive adhesive, silicone or acrylic with a thickness ranging from 15 to 25 um.
[0018] Beneficial effects:
[0019] 1. This patent adopts a five-layer structure with higher production efficiency. When in use, tear off the lower PET release layer and stick it on the surface of the mobile phone screen. Then tear off the upper PET release layer and use UV light to irradiate the double-curing adhesive layer to further solidify and shape it on the surface of the mobile phone, so as to better fit the curved screen mobile phone and provide better protection.
[0020] 2. Normal protective films or ordinary UV post-curing protective films on the market currently all use base films as carriers. However, the flagship mobile phones on the market now all have optical under-screen fingerprint unlocking. The base film itself is a biaxially stretched film, and the base film has irregular birefringence inside, which causes irregular refraction phase difference after the light under the screen comes out, resulting in a certain deviation in the under-screen fingerprint unlocking, causing unlocking risks. The dual-curing adhesive layer of this product can be directly coated with a self-repairing coating and a pressure-sensitive adhesive coating, and the base film can be directly removed, so that this protective film will not have optical phase difference refraction, meeting all under-screen fingerprint unlocking requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a schematic structural diagram of a protective film according to an embodiment;
[0022] Upper PET release layer: 110; self-healing coating: 120; dual-curing adhesive layer: 130; pressure-sensitive adhesive layer: 140; upper and lower PET release layers: 150. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0024] The embodiment of the present invention provides a method for preparing a polyamide material with high heat dissipation and high strength, the method mainly comprising the following steps:
[0025] S1, preparing the dual-curing adhesive layer raw materials according to the mass ratio;
[0026] Prepare the raw materials according to the mass ratio: modified polyurethane acrylate: 10-20 parts, special functional group polyurethane acrylate: 20-30 parts, isobornyl acrylate: 10-20 parts, cycloaliphatic acrylate: 10-20 parts, 4-hydroxybutyl acrylate: 10-20 parts, diisocyanate-terminated polyester polyol curing agent: 1-5 parts, 1-hydroxycyclohexyl phenyl ketone: 2-3 parts, diphenyl-(2,4,6-trivalent benzoyl)phosphine oxide: 2-3 parts;
[0027] S2, a dual-cured adhesive layer is obtained by supercritical treatment;
[0028] Stirring the dual-curing adhesive layer raw materials to mix the solution;
[0029] Performing vacuum degassing on the mixed solution to obtain a pre-solution;
[0030] The pre-solution is subjected to supercritical treatment to obtain a dual-cured adhesive layer;
[0031] S3,,superimpose according to the designed structure to obtain a mobile phone protective film;
[0032] From top to bottom: PET release layer, self-healing coating, dual-curing adhesive layer, pressure-sensitive adhesive layer, PET release layer;
[0033] As an embodiment, the following content of the embodiments of the present invention gives several specific examples of the above-mentioned method for preparing a polyamide material with high heat dissipation and high strength, such as Example 1, Example 2, Example 3 and Examples 1-6 for comparison and explanation.
[0034] Embodiment 1:
[0035] S1, configure the dual-curing adhesive layer raw materials according to the mass ratio
[0036] Prepare the raw materials according to the mass ratio: modified polyurethane acrylate: 10 parts, special functional group polyurethane acrylate: 20 parts, isobornyl acrylate: 10 parts, cycloaliphatic acrylate: 10 parts, 4-hydroxybutyl acrylate: 10 parts, diisocyanate-terminated polyester polyol curing agent: 1 part, 1-hydroxycyclohexyl phenyl ketone: 2 parts, diphenyl-(2,4,6-trivalent benzoyl)phosphine: 2 parts;
[0037] S2, dual-cured adhesive layer obtained by supercritical treatment
[0038] The mixed solution was placed in a vacuum degassing device for vacuum degassing to obtain a pre-solution, the vacuum degree was 0.1 Pa, and the pressure holding time was 20 min;
[0039] The pre-solution was subjected to supercritical treatment to obtain a dual-cured adhesive layer at a treatment temperature of 100°C, a pressure of 20 MPa, and a time of 2 h. The pore density of the dual-cured adhesive layer was 10 12 / cm 3 , the light transmittance of the dual-cured adhesive layer is greater than 90%, the haze is less than 2%, and the thickness range is 0.08mm;
[0040] S3, stacking according to the designed structure to obtain a mobile phone protective film
[0041] From top to bottom: PET release layer, self-healing coating, dual-curing adhesive layer, pressure-sensitive adhesive layer, PET release layer;
[0042] Furthermore, the upper PET release layer and the lower PET release layer are both release films, the thickness of the release films is 40um, and the light transmittance is greater than 88%;
[0043] Furthermore, the release film is obtained by mixing raw materials, the mixing method is vacuum ball milling + vacuum degassing treatment, the ball milling speed is 100 rpm, and TEMOPO-modified nanocellulose is added to the raw materials before ball milling, and the cellulose has a length of 200 nm and a diameter of 3 nm;
[0044] Furthermore, the self-repairing coating is one of a polyurethane elastic coating or a UV elastic self-repairing coating, the self-repairing coating is modified by a silane coupling agent KH550, the material has an adhesive strength of 0.7 MPa, and a thermal weight loss temperature of 230°C;
[0045] Furthermore, the self-repairing coating is coated on the double-cured adhesive layer by a coating process, the thickness of the self-repairing coating is 15 um, the coating process refers to ultrasonic thermal coating, the ultrasonic frequency is 0.5 KHz, the coating temperature is 60° C., and the processing time is 10 min;
[0046] Furthermore, the pressure-sensitive adhesive layer is one of polyurethane pressure-sensitive adhesive, silicone or acrylic with a thickness ranging from 15 um.
[0047] Embodiment 2:
[0048] S1, configure the dual-curing adhesive layer raw materials according to the mass ratio
[0049] Prepare the raw materials according to the mass ratio: modified polyurethane acrylate: 20 parts, special functional group polyurethane acrylate: 30 parts, isobornyl acrylate: 20 parts, cycloaliphatic acrylate: 20 parts, 4-hydroxybutyl acrylate: 20 parts, diisocyanate-terminated polyester polyol curing agent: 5 parts, 1-hydroxycyclohexyl phenyl ketone: 3 parts, diphenyl-(2,4,6-trivalent benzoyl)phosphine: 3 parts;
[0050] S2, dual-cured adhesive layer obtained by supercritical treatment
[0051] The mixed solution was placed in a vacuum degassing device for vacuum degassing to obtain a pre-solution, the vacuum degree was 0.5 Pa, and the pressure holding time was 40 min;
[0052] The pre-solution was subjected to supercritical treatment to obtain a dual-cured adhesive layer at a treatment temperature of 130°C, a pressure of 30 MPa, and a time of 4 h. The pore density of the dual-cured adhesive layer was 10 15 / cm 3 , the light transmittance of the dual-cured adhesive layer is greater than 90%, the haze is less than 2%, and the thickness range is 0.12mm;
[0053] S3, stacking according to the designed structure to obtain a mobile phone protective film
[0054] From top to bottom: PET release layer, self-healing coating, dual-curing adhesive layer, pressure-sensitive adhesive layer, PET release layer;
[0055] Furthermore, the upper PET release layer and the lower PET release layer are both release films, the thickness of the release films is 60um, and the light transmittance is greater than 88%;
[0056] Furthermore, the release film is obtained by mixing raw materials, the mixing method is vacuum ball milling + vacuum degassing treatment, the ball milling speed is 200 rpm, and TEMOPO-modified nanocellulose is added to the raw materials before ball milling, and the cellulose has a length of 600 nm and a diameter of 10 nm;
[0057] Furthermore, the self-repairing coating is one of a polyurethane elastic coating or a UV elastic self-repairing coating, the self-repairing coating is modified by a silane coupling agent KH550, the material has an adhesive strength of 1.1 MPa, and a thermal weight loss temperature of 270°C;
[0058] Furthermore, the self-repairing coating is coated on the double-cured adhesive layer by a coating process, the thickness of the self-repairing coating is 20 um, the coating process refers to ultrasonic thermal coating, the ultrasonic frequency is 0.8 KHz, the coating temperature is 100° C., and the processing time is 30 min;
[0059] Furthermore, the pressure-sensitive adhesive layer is one of polyurethane pressure-sensitive adhesive, silicone or acrylic with a thickness ranging from 15 to 25 um.
[0060] Embodiment 3:
[0061] S1, prepare the dual-curing adhesive layer raw materials according to the mass ratio
[0062] Prepare the raw materials according to the mass ratio: modified polyurethane acrylate: 15 parts, special functional group polyurethane acrylate: 25 parts, isobornyl acrylate: 15 parts, cycloaliphatic acrylate: 15 parts, 4-hydroxybutyl acrylate: 15 parts, diisocyanate-terminated polyester polyol curing agent: 3 parts, 1-hydroxycyclohexyl phenyl ketone: 2 parts, diphenyl-(2,4,6-trivalent benzoyl)phosphine: 2 parts;
[0063] S2, dual-cured adhesive layer obtained by supercritical treatment
[0064] The mixed solution was placed in a vacuum degassing device for vacuum degassing to obtain a pre-solution, the vacuum degree was 0.3 Pa, and the pressure holding time was 30 min;
[0065] The pre-solution was subjected to supercritical treatment to obtain a dual-cured adhesive layer at a treatment temperature of 120°C, a pressure of 25 MPa, and a time of 3 h. The pore density of the dual-cured adhesive layer was 10 14 / cm 3 , the light transmittance of the dual-cured adhesive layer is greater than 90%, the haze is less than 2%, and the thickness range is 0.1mm;
[0066] S3, stacking according to the designed structure to obtain a mobile phone protective film
[0067] From top to bottom: PET release layer, self-healing coating, dual-curing adhesive layer, pressure-sensitive adhesive layer, PET release layer;
[0068] Furthermore, the upper PET release layer and the lower PET release layer are both release films, the thickness of the release films is 50um, and the light transmittance is greater than 88%;
[0069] Furthermore, the release film is obtained by mixing raw materials, the mixing method is vacuum ball milling + vacuum degassing treatment, the ball milling speed is 150rpm, and TEMOPO-modified nanocellulose is added to the raw materials before ball milling, and the cellulose has a length of 400nm and a diameter of 7nm;
[0070] Furthermore, the self-repairing coating is one of a polyurethane elastic coating or a UV elastic self-repairing coating, the self-repairing coating is modified by a silane coupling agent KH550, the material has an adhesive strength of 0.9 MPa, and a thermal weight loss temperature of 250°C;
[0071] Furthermore, the self-repairing coating is coated on the double-cured adhesive layer by a coating process, the thickness of the self-repairing coating is 17um, the coating process refers to ultrasonic thermal coating, the ultrasonic frequency is 0.7KHz, the coating temperature is 80°C, and the processing time is 20min;
[0072] Furthermore, the pressure-sensitive adhesive layer is one of polyurethane pressure-sensitive adhesive, silicone or acrylic with a thickness ranging from 20 um.
[0073] Comparative Example 1:
[0074] S1, prepare the dual-curing adhesive layer raw materials according to the mass ratio
[0075] Prepare the raw materials according to the mass ratio: modified polyurethane acrylate: 15 parts, special functional group polyurethane acrylate: 25 parts, isobornyl acrylate: 15 parts, cycloaliphatic acrylate: 15 parts, 4-hydroxybutyl acrylate: 15 parts, diisocyanate-terminated polyester polyol curing agent: 3 parts, 1-hydroxycyclohexyl phenyl ketone: 2 parts, diphenyl-(2,4,6-trivalent benzoyl)phosphine: 2 parts;
[0076] S2, dual-cured adhesive layer obtained by supercritical treatment
[0077] The mixed solution was placed in a vacuum degassing device for vacuum degassing to obtain a pre-solution, the vacuum degree was 0.3 Pa, and the pressure holding time was 30 min;
[0078] The pre-solution was subjected to supercritical treatment to obtain a dual-cured adhesive layer at a treatment temperature of 120°C, a pressure of 3 MPa, and a time of 3 h. The pore density of the dual-cured adhesive layer was 10 3 / cm 3 , the light transmittance of the dual-cured adhesive layer is greater than 90%, the haze is less than 2%, and the thickness range is 0.1mm;
[0079] S3, stacking according to the designed structure to obtain a mobile phone protective film
[0080] From top to bottom: PET release layer, self-healing coating, dual-curing adhesive layer, pressure-sensitive adhesive layer, PET release layer;
[0081] Furthermore, the upper PET release layer and the lower PET release layer are both release films, the thickness of the release films is 50um, and the light transmittance is greater than 88%;
[0082] Furthermore, the release film is obtained by mixing raw materials, the mixing method is vacuum ball milling + vacuum degassing treatment, the ball milling speed is 150rpm, and TEMOPO-modified nanocellulose is added to the raw materials before ball milling, and the cellulose has a length of 400nm and a diameter of 7nm;
[0083] Furthermore, the self-repairing coating is one of a polyurethane elastic coating or a UV elastic self-repairing coating, the self-repairing coating is modified by a silane coupling agent KH550, the material has an adhesive strength of 0.9 MPa, and a thermal weight loss temperature of 250°C;
[0084] Furthermore, the self-repairing coating is coated on the double-cured adhesive layer by a coating process, the thickness of the self-repairing coating is 17um, the coating process refers to ultrasonic thermal coating, the ultrasonic frequency is 0.7KHz, the coating temperature is 80°C, and the processing time is 20min;
[0085] Furthermore, the pressure-sensitive adhesive layer is one of polyurethane pressure-sensitive adhesive, silicone or acrylic with a thickness ranging from 20 um.
[0086] Comparative Example 2:
[0087] S1, configure the dual-curing adhesive layer raw materials according to the mass ratio
[0088] Prepare the raw materials according to the mass ratio: modified polyurethane acrylate: 15 parts, special functional group polyurethane acrylate: 25 parts, isobornyl acrylate: 15 parts, cycloaliphatic acrylate: 15 parts, 4-hydroxybutyl acrylate: 15 parts, diisocyanate-terminated polyester polyol curing agent: 3 parts, 1-hydroxycyclohexyl phenyl ketone: 2 parts, diphenyl-(2,4,6-trivalent benzoyl)phosphine: 2 parts;
[0089] S2, dual-cured adhesive layer obtained by supercritical treatment
[0090] The mixed solution was placed in a vacuum degassing device for vacuum degassing to obtain a pre-solution, the vacuum degree was 0.3 Pa, and the pressure holding time was 30 min;
[0091] The pre-solution was subjected to supercritical treatment to obtain a dual-cured adhesive layer at a treatment temperature of 120°C, a pressure of 25 MPa, and a time of 3 h. The pore density of the dual-cured adhesive layer was 10 14 / cm 3 , the light transmittance of the dual-cured adhesive layer is greater than 90%, the haze is less than 2%, and the thickness range is 0.1mm;
[0092] S3, stacking according to the designed structure to obtain a mobile phone protective film
[0093] From top to bottom: PET release layer, self-healing coating, dual-curing adhesive layer, pressure-sensitive adhesive layer, PET release layer;
[0094] Furthermore, the upper PET release layer and the lower PET release layer are both release films;
[0095] Furthermore, the release film has a thickness of 50 um and a light transmittance greater than 88%. The release film is obtained by mixing raw materials, the mixing method is vacuum ball milling + vacuum degassing treatment, and the ball milling speed is 150 rpm;
[0096] Furthermore, the self-repairing coating is one of a polyurethane elastic coating or a UV elastic self-repairing coating, the self-repairing coating is modified by a silane coupling agent KH550, the material has an adhesive strength of 0.9 MPa, and a thermal weight loss temperature of 250°C;
[0097] Furthermore, the self-repairing coating is coated on the double-cured adhesive layer by a coating process, the thickness of the self-repairing coating is 17um, the coating process refers to ultrasonic thermal coating, the ultrasonic frequency is 0.7KHz, the coating temperature is 80°C, and the processing time is 20min;
[0098] Furthermore, the pressure-sensitive adhesive layer is one of polyurethane pressure-sensitive adhesive, silicone or acrylic with a thickness ranging from 20 um.
[0099] Comparative Example 3:
[0100] S1, prepare the dual-curing adhesive layer raw materials according to the mass ratio
[0101] Prepare the raw materials according to the mass ratio: modified polyurethane acrylate: 15 parts, special functional group polyurethane acrylate: 25 parts, isobornyl acrylate: 15 parts, cycloaliphatic acrylate: 15 parts, 4-hydroxybutyl acrylate: 15 parts, diisocyanate-terminated polyester polyol curing agent: 3 parts, 1-hydroxycyclohexyl phenyl ketone: 2 parts, diphenyl-(2,4,6-trivalent benzoyl)phosphine: 2 parts;
[0102] S2, dual-cured adhesive layer obtained by supercritical treatment
[0103] The mixed solution was placed in a vacuum degassing device for vacuum degassing to obtain a pre-solution, the vacuum degree was 0.3 Pa, and the pressure holding time was 30 min;
[0104] The pre-solution was subjected to supercritical treatment to obtain a dual-cured adhesive layer at a treatment temperature of 120°C, a pressure of 25 MPa, and a time of 3 h. The pore density of the dual-cured adhesive layer was 10 14 / cm 3 , the light transmittance of the dual-cured adhesive layer is greater than 90%, the haze is less than 2%, and the thickness range is 0.1mm;
[0105] S3, stacking according to the designed structure to obtain a mobile phone protective film
[0106] From top to bottom: PET release layer, self-healing coating, dual-curing adhesive layer, pressure-sensitive adhesive layer, PET release layer;
[0107] Furthermore, the upper PET release layer and the lower PET release layer are both release films, the thickness of the release films is 50um, and the light transmittance is greater than 88%;
[0108] Furthermore, the release film is obtained by mixing raw materials, the mixing method is vacuum ball milling + vacuum degassing treatment, the ball milling speed is 150rpm, and TEMOPO-modified nanocellulose is added to the raw materials before ball milling, and the cellulose length is 20nm and the diameter is 7nm;
[0109] Furthermore, the self-repairing coating is one of a polyurethane elastic coating or a UV elastic self-repairing coating, the self-repairing coating is modified by a silane coupling agent KH550, the material has an adhesive strength of 0.9 MPa, and a thermal weight loss temperature of 250°C;
[0110] Furthermore, the self-repairing coating is coated on the double-cured adhesive layer by a coating process, the thickness of the self-repairing coating is 17um, the coating process refers to ultrasonic thermal coating, the ultrasonic frequency is 0.7KHz, the coating temperature is 80°C, and the processing time is 20min;
[0111] Furthermore, the pressure-sensitive adhesive layer is one of polyurethane pressure-sensitive adhesive, silicone or acrylic with a thickness ranging from 20 um.
[0112] Comparative Example 4:
[0113] S1, prepare the dual-curing adhesive layer raw materials according to the mass ratio
[0114] Prepare the raw materials according to the mass ratio: modified polyurethane acrylate: 15 parts, special functional group polyurethane acrylate: 25 parts, isobornyl acrylate: 15 parts, cycloaliphatic acrylate: 15 parts, 4-hydroxybutyl acrylate: 15 parts, diisocyanate-terminated polyester polyol curing agent: 3 parts, 1-hydroxycyclohexyl phenyl ketone: 2 parts, diphenyl-(2,4,6-trivalent benzoyl)phosphine: 2 parts;
[0115] S2, dual-cured adhesive layer obtained by supercritical treatment
[0116] The mixed solution was placed in a vacuum degassing device for vacuum degassing to obtain a pre-solution, the vacuum degree was 0.3 Pa, and the pressure holding time was 30 min;
[0117] The pre-solution was subjected to supercritical treatment to obtain a dual-cured adhesive layer at a treatment temperature of 120°C, a pressure of 25 MPa, and a time of 3 h. The pore density of the dual-cured adhesive layer was 10 14 / cm 3 , the light transmittance of the dual-cured adhesive layer is greater than 90%, the haze is less than 2%, and the thickness range is 0.1mm;
[0118] S3, stacking according to the designed structure to obtain a mobile phone protective film
[0119] From top to bottom: PET release layer, self-healing coating, dual-curing adhesive layer, pressure-sensitive adhesive layer, PET release layer;
[0120] Furthermore, the upper PET release layer and the lower PET release layer are both release films, the thickness of the release films is 50um, and the light transmittance is greater than 88%;
[0121] Furthermore, the release film is obtained by mixing raw materials, the mixing method is vacuum ball milling + vacuum degassing treatment, the ball milling speed is 150rpm, and TEMOPO-modified nanocellulose is added to the raw materials before ball milling, and the cellulose has a length of 400nm and a diameter of 7nm;
[0122] Further, the self-repairing coating is one of a polyurethane elastic coating or a UV elastic self-repairing coating;
[0123] Furthermore, the self-repairing coating is coated on the double-cured adhesive layer by a coating process, the thickness of the self-repairing coating is 17um, the coating process refers to ultrasonic thermal coating, the ultrasonic frequency is 0.7KHz, the coating temperature is 80°C, and the processing time is 20min;
[0124] Furthermore, the pressure-sensitive adhesive layer is one of polyurethane pressure-sensitive adhesive, silicone or acrylic with a thickness ranging from 20 um.
[0125] Comparative Example 5:
[0126] S1, prepare the dual-curing adhesive layer raw materials according to the mass ratio
[0127] Prepare the raw materials according to the mass ratio: modified polyurethane acrylate: 15 parts, special functional group polyurethane acrylate: 25 parts, isobornyl acrylate: 15 parts, cycloaliphatic acrylate: 15 parts, 4-hydroxybutyl acrylate: 15 parts, diisocyanate-terminated polyester polyol curing agent: 3 parts, 1-hydroxycyclohexyl phenyl ketone: 2 parts, diphenyl-(2,4,6-trivalent benzoyl)phosphine: 2 parts;
[0128] S2, dual-cured adhesive layer obtained by supercritical treatment
[0129] The mixed solution was placed in a vacuum degassing device for vacuum degassing to obtain a pre-solution, the vacuum degree was 0.3 Pa, and the pressure holding time was 30 min;
[0130] The pre-solution was subjected to supercritical treatment to obtain a dual-cured adhesive layer at a treatment temperature of 120°C, a pressure of 25 MPa, and a time of 3 h. The pore density of the dual-cured adhesive layer was 10 14 / cm 3 , the light transmittance of the dual-cured adhesive layer is greater than 90%, the haze is less than 2%, and the thickness range is 0.1mm;
[0131] S3, stacking according to the designed structure to obtain a mobile phone protective film
[0132] From top to bottom: PET release layer, self-healing coating, dual-curing adhesive layer, pressure-sensitive adhesive layer, PET release layer;
[0133] Furthermore, the upper PET release layer and the lower PET release layer are both release films, the thickness of the release films is 50um, and the light transmittance is greater than 88%;
[0134] Furthermore, the release film is obtained by mixing raw materials, the mixing method is vacuum ball milling + vacuum degassing treatment, the ball milling speed is 150rpm, and TEMOPO-modified nanocellulose is added to the raw materials before ball milling, and the cellulose has a length of 400nm and a diameter of 7nm;
[0135] Furthermore, the self-repairing coating is one of a polyurethane elastic coating or a UV elastic self-repairing coating, the self-repairing coating is modified by a silane coupling agent KH550, the material has an adhesive strength of 0.9 MPa, and a thermal weight loss temperature of 250°C;
[0136] Furthermore, the self-repairing coating is applied on top of the dual-curing adhesive layer by a common coating process, and the thickness of the self-repairing coating is 17 um;
[0137] Furthermore, the pressure-sensitive adhesive layer is one of polyurethane pressure-sensitive adhesive, silicone or acrylic with a thickness ranging from 20 um.
[0138] Comparative Example 6:
[0139] S1, configure the dual-curing adhesive layer raw materials according to the mass ratio
[0140] Prepare the raw materials according to the mass ratio: modified polyurethane acrylate: 15 parts, special functional group polyurethane acrylate: 25 parts, isobornyl acrylate: 15 parts, cycloaliphatic acrylate: 15 parts, 4-hydroxybutyl acrylate: 15 parts, diisocyanate-terminated polyester polyol curing agent: 3 parts, 1-hydroxycyclohexyl phenyl ketone: 2 parts, diphenyl-(2,4,6-trivalent benzoyl)phosphine: 2 parts;
[0141] S2, dual-cured adhesive layer obtained by supercritical treatment
[0142] The mixed solution was placed in a vacuum degassing device for vacuum degassing to obtain a pre-solution, the vacuum degree was 0.3 Pa, and the pressure holding time was 30 min;
[0143] The pre-solution was subjected to supercritical treatment to obtain a dual-cured adhesive layer at a treatment temperature of 120°C, a pressure of 25 MPa, and a time of 3 h. The pore density of the dual-cured adhesive layer was 10 14 / cm 3 , the light transmittance of the dual-cured adhesive layer is greater than 90%, the haze is less than 2%, and the thickness range is 0.1mm;
[0144] S3, stacking according to the designed structure to obtain a mobile phone protective film
[0145] From top to bottom: PET release layer, self-healing coating, dual-curing adhesive layer, pressure-sensitive adhesive layer, PET release layer;
[0146] Furthermore, the upper PET release layer and the lower PET release layer are both release films, the thickness of the release films is 5um, and the light transmittance is greater than 88%;
[0147] Furthermore, the release film is obtained by mixing raw materials, the mixing method is vacuum ball milling + vacuum degassing treatment, the ball milling speed is 150rpm, and TEMOPO-modified nanocellulose is added to the raw materials before ball milling, and the cellulose has a length of 400nm and a diameter of 7nm;
[0148] Furthermore, the self-repairing coating is one of a polyurethane elastic coating or a UV elastic self-repairing coating, the self-repairing coating is modified by a silane coupling agent KH550, the material has an adhesive strength of 0.9 MPa, and a thermal weight loss temperature of 250°C;
[0149] Furthermore, the self-repairing coating is coated on the double-cured adhesive layer by a coating process, the thickness of the self-repairing coating is 17um, the coating process refers to ultrasonic thermal coating, the ultrasonic frequency is 0.7KHz, the coating temperature is 80°C, and the processing time is 20min;
[0150] Furthermore, the pressure-sensitive adhesive layer is one of polyurethane pressure-sensitive adhesive, silicone or acrylic with a thickness ranging from 20 um.
[0151] Table 1:
[0152] project Light transmittance Wear resistance Tensile Strength Example 1 84% excellent >25MPa Example 2 87% excellent >25MPa Example 3 94% excellent >25MPa Comparative Example 1 74% good >20MPa Comparative Example 2 86% good <15MPa Comparative Example 3 84% generally >20MPa Comparative Example 4 85% good >15MPa Comparative Example 5 79% good >15MPa Comparative Example 6 86% Poor <5MPa
[0153] From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 1 in Table 1, it can be found that the light transmittance, wear resistance and tensile strength of Examples 1, 2 and 3 compared with Comparative Example 1 are all reduced, which shows that after the dual-cured adhesive layer is subjected to supercritical treatment, there is a significant gain in improving the light transmittance of the material, and the high porosity will also increase the specific strength of the material; from the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 2 in Table 1, it can be found that the tensile strength of Examples 1, 2 and 3 compared with Comparative Example 2 is significantly reduced, which shows that the addition of TEMOPO-modified nanocellulose has an effect on improving the material strength of the release film, and it can play a good tensile effect; from the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 3 in Table 1, it can be found that the wear resistance and tensile strength of Examples 1, 2 and 3 compared with Comparative Example 3 are all reduced, which shows that when the size of the nanocellulose modified by TEMOPO is reduced, its effect on the chimeric effect of the material will be reduced, Thereby affecting the tensile strength of the material; from the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 4 in Table 1, it can be found that the tensile strength of Examples 1, 2, 3 compared with Comparative Example 4 is significantly reduced, indicating that the modification of the self-repairing coating with silane coupling agent KH550 is beneficial to improving the bonding effect of the material; from the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 5 in Table 1, it can be found that the transmittance, wear resistance and tensile strength of Examples 1, 2, 3 compared with Comparative Example 5 are all reduced, indicating that after the self-repairing coating is heated and ultrasonically coated, the bonding strength between the coating and the substrate is improved, and the pores and air holes that appear in general coating are eliminated; from the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 6 in Table 1, it can be found that the wear resistance and tensile strength of Examples 1, 2, 3 compared with Comparative Example 6 are abnormally reduced, indicating that reducing the thickness of the upper and lower PET release layers is not conducive to the overall performance of the material, and it is not conducive to improving the strength of the material.
[0154] Although the embodiments of the present application have been shown and described above, it is understood that the above embodiments are exemplary and cannot be construed as limitations on the present application. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A method for preparing a dual-curing adhesive layer and a mobile phone protective film thereof, characterized in that: include: Configure the dual-curing adhesive layer raw materials according to the mass ratio; A dual-cured adhesive layer is obtained by supercritical treatment; The mobile phone protective film is obtained by stacking according to the designed structure.
2. The method for preparing a dual-curing adhesive layer and a mobile phone protective film thereof according to claim 1, characterized in that: The step of configuring the dual-curing adhesive layer raw materials according to the mass ratio includes: Prepare the raw materials according to the mass ratio: modified polyurethane acrylate: 10-20 parts, special functional group polyurethane acrylate: 20-30 parts, isobornyl acrylate: 10-20 parts, cycloaliphatic acrylate: 10-20 parts, 4-hydroxybutyl acrylate: 10-20 parts, diisocyanate-terminated polyester polyol curing agent: 1-5 parts, 1-hydroxycyclohexyl phenyl ketone: 2-3 parts, diphenyl-(2,4,6-trivalent benzoyl)phosphine oxide: 2-3 parts; The step of obtaining the dual-cured adhesive layer by supercritical treatment comprises: Stirring the dual-curing adhesive layer raw materials to mix the solution; Performing vacuum degassing on the mixed solution to obtain a pre-solution; The pre-solution is subjected to supercritical treatment to obtain a dual-cured adhesive layer; The step of obtaining the mobile phone protective film by stacking according to the designed structure comprises: From top to bottom: PET release layer, self-healing coating, dual-curing adhesive layer, pressure-sensitive adhesive layer, and PET release layer.
3. The method for preparing a polyamide material with high heat dissipation and high strength according to claim 2, characterized in that: The step of stirring and degassing the dual-curing adhesive layer raw material to obtain a pre-solution comprises: Modified polyurethane acrylate, special functional group polyurethane acrylate, isobornyl acrylate, cycloaliphatic acrylate, 4-hydroxybutyl acrylate, diisocyanate-terminated polyester polyol curing agent, 1-hydroxycyclohexyl phenyl ketone, and diphenyl-(2,4,6-trivalent benzoyl)phosphine are mixed and stirred to obtain a mixed solution at a stirring speed of 400-600 rpm for 30-60 minutes.
4. The method for preparing a polyamide material with high heat dissipation and high strength according to claim 2, characterized in that: The step of vacuum degassing the mixed solution to obtain the pre-solution comprises: The mixed solution is placed in a vacuum degassing device for vacuum degassing to obtain a pre-solution, the vacuum degree is 0.1-0.5Pa, and the pressure holding time is 20-40min.
5. The method for preparing a polyamide material with high heat dissipation and high strength according to claim 2, characterized in that: The step of subjecting the pre-solution to supercritical treatment to obtain a dual-cured adhesive layer comprises: The pre-solution is subjected to supercritical treatment to obtain a dual-cured adhesive layer at a treatment temperature of 100°C-130°C, a pressure of 20-30MPa, and a time of 2-4h. The pore density of the dual-cured adhesive layer is 10 12 -10 15 / cm 3 The light transmittance of the cured adhesive layer is greater than 90%, the haze is less than 2%, and the thickness range is 0.08-0.12mm.
6. The method for preparing a dual-curing adhesive layer and a mobile phone protective film thereof according to claim 2, characterized in that: The upper PET release layer and the lower PET release layer are both release films, the thickness of the release films is 40-60um, and the light transmittance is greater than 88%.
7. The method for preparing a dual-curing adhesive layer and a mobile phone protective film thereof according to claim 6, characterized in that: The release film is obtained by mixing raw materials by vacuum ball milling and vacuum degassing treatment, the ball milling speed is 100-200rpm, and TEMOPO-modified nanocellulose is added to the raw materials before ball milling, the cellulose length is 200-600nm, and the diameter is 3-10nm.
8. The method for preparing a dual-curing adhesive layer and a mobile phone protective film thereof according to claim 2, characterized in that: The self-repairing coating is a polyurethane elastic coating or a UV elastic self-repairing coating. The self-repairing coating is modified by a silane coupling agent KH550. The material has an adhesive strength of 0.7-1.1 MPa and a thermal weight loss temperature of 230-270°C.
9. The method for preparing a dual-curing adhesive layer and a mobile phone protective film thereof according to claim 8, characterized in that: The self-healing coating is coated on the double-cured adhesive layer through a coating process. The thickness of the self-healing coating is 15-20um. The coating process refers to ultrasonic thermal coating. The ultrasonic frequency is 0.5-0.8KHz, the coating temperature is 60-100°C, and the processing time is 10-30min.
10. The method for preparing a dual-curing adhesive layer and a mobile phone protective film thereof according to claim 2, characterized in that: The pressure-sensitive adhesive layer is one of polyurethane pressure-sensitive adhesive, silica gel or acrylic with a thickness ranging from 15 to 25 μm.