Co-extrusion adhesive film capable of reducing subfissure and white overflow and preparation method of co-extrusion adhesive film
The photovoltaic module is solved by using a coextruded adhesive film of a pre-crosslinked white EVA film layer and a transparent EVA film layer without irradiation, combined with unsaturated carboxylic acid ester of a single carbon carbon double bond in a photovoltaic module. The problems of overflow and cracking in lamination simplify the production process and improve the reliability of components.
Patent Information
- Application Number
- CN202411085714.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
During the lamination process of photovoltaic modules, uncrosslinked EVA film causes whitening and hidden cracking problems. The introduction of hard isolation layers in existing solutions leads to complex production processes and high cost, and poor bonding performance, which affects the impact of Component reliability.
A coextruded film consisting of a pre-crosslinked white EVA film layer and a transparent EVA film layer that does not cross-link with irradiation is adopted. The transparent EVA film layer contains unsaturated carboxylic acid ester with a single carbon carbon double bond, and is coextruded. Forming and irradiation treatment to reduce fluidity and hidden cracking risks.
The production of co-extruded adhesive films under existing equipment is realized, reducing the risk of overflow and cracking, simplifying the process, and improving the reliability and production efficiency of components.
Smart Images

Figure CN118995074A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adhesive films, and in particular relates to a co-extruded adhesive film capable of reducing hidden cracks and white overflow and a preparation method thereof. Background Art
[0002] In order to increase the power of the modules, the photovoltaic industry uses white fillers to reflect the light that passes through the gaps between the cells and the infrared light that passes through the cells to increase the light absorption of the modules. As a result, white EVA films are developed to encapsulate the back of the modules. Since the uncross-linked EVA films have good fluidity, the white EVA films overflow to the front of the cells during module lamination, covering the front of the cells, which leads to power attenuation and poor appearance of the modules. Therefore, when using white EVA films, irradiation equipment will be used to irradiate the films in advance, and the white films will be pre-cross-linked to reduce the fluidity of the white EVA films and reduce the risk of white overflow. The pre-cross-linking degree of the white films generally needs to be controlled at 25%-40%. Although the method of reducing fluidity by irradiation can reduce the risk of white film white overflow, the pre-cross-linked EVA films become hard, the buffer is reduced, and the filling effect is poor, making it difficult to fill the gap between the cells and the bends of the solder strips, which greatly increases the defect of hidden cracks in the cells during lamination of the white EVA films. In response to the above problems, some people in the industry use isolation methods to improve this problem. Chinese patent CN 203013768 U discloses a highly reflective EVA film for photovoltaic modules, which adds a non-woven fabric layer between the transparent EVA layer and the white reflective EVA layer as an isolation layer to solve the problems of white overflow and hidden cracks; Chinese patent CN219363539 U discloses a composite white film and photovoltaic module for photovoltaic modules, which adds a polyester fiber mesh cloth between the transparent EVA layer and the white reflective EVA layer as an isolation layer to solve the lamination problem. The above two solutions introduce a hard isolation layer in the middle of the EVA, which makes it impossible to produce such films with the current extrusion process. It is necessary to adopt a double-sided coating process for production, which requires additional equipment. The cost of the double-sided coating process is also higher than the current single composite extrusion cost; in addition, due to the introduction of a third substance in EVA, the bonding performance between EVA and the isolation layer is not as good as that of EVA alone, and delamination problems are prone to occur during aging, affecting the reliability of the module. Contents of the invention
[0003] In order to solve the above technical problems, the present invention provides a co-extruded adhesive film for reducing hidden cracks and white overflow and a preparation method thereof. When the co-extruded adhesive film is used, the transparent EVA film layer side of the co-extruded adhesive film contacts the surface of the photovoltaic module. There will be no hidden crack problem during lamination, and there will be no white overflow on the surface of the photovoltaic module.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0005] A co-extruded adhesive film for reducing hidden cracks and white overflow, the co-extruded adhesive film is composed of a white EVA film layer and a transparent EVA film layer; the white EVA film layer is pre-crosslinked by irradiation; the raw material of the transparent EVA film layer contains an unsaturated carboxylic acid ester with a single carbon-carbon double bond; the transparent EVA film layer is not crosslinked by irradiation.
[0006] In the transparent EVA film layer, the weight ratio of the unsaturated carboxylic acid ester with a single carbon-carbon double bond to the EVA resin is 0.3-0.7:100.
[0007] The unsaturated carboxylic acid ester with a single carbon-carbon double bond is any one or more of methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, and butyl acrylate.
[0008] The thickness ratio of the white EVA film layer to the transparent EVA film layer is 3:2.
[0009] When the white EVA film layer is irradiated for pre-crosslinking, the irradiation pulling speed is 15-25 m / min, and the irradiation beam current is 35-40 mA.
[0010] The white EVA film layer uses EVA resin with a melt index of 3-15g / 10min as the main material.
[0011] The transparent EVA film layer uses EVA resin with a melt index of 15-50g / 10min as the main material.
[0012] The raw materials of the white EVA film layer are the following substances in weight: 100 parts of EVA resin with a melt index of 3-15g / 10min, 0.5-1.5 parts of a crosslinking agent, 0.2-1.0 parts of a coupling agent, 1.0-2.0 parts of a co-crosslinking agent, 0.2-1.0 parts of an antioxidant, 0.1-1.0 parts of an acid scavenger, and 5-10 parts of a white filler.
[0013] The raw materials of the transparent EVA film layer are the following substances in weight: 100 parts of EVA resin with a melt index of 15-50g / 10min, 0.5-1 parts of a crosslinking agent, 0.2-0.7 parts of a coupling agent, 1.0-2.0 parts of a co-crosslinking agent, 0.2-0.5 parts of an antioxidant, 0.1-0.5 parts of an acid scavenger, and 0.3-0.7 parts of an unsaturated carboxylic acid ester with a single carbon-carbon double bond.
[0014] The crosslinking agent is a peroxide crosslinking agent, which is one or more of tert-butyl peroxy-2-ethylhexanoate, tert-amyl peroxy (2-ethylhexyl) carbonate, 1,1-(ditert-butyl peroxide) 3,3,5-trimethylcyclohexane, diisopropylbenzene peroxide, di-tert-butyl peroxyisopropylbenzene, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.
[0015] The coupling agent is one or more of γ-methacryloxypropyltrimethoxysilane, vinyltri(2-methoxyethoxy)silane, vinyltrimethylsilane, and 3-aminopropyltriethoxysilane.
[0016] The auxiliary cross-linking agent is one or more of triallyl cyanurate, triallyl isocyanurate, ethoxylated trimethylolpropane triacrylate, trimethylolpropane triacrylate, divinylbenzene, and 1,2-diallyl phthalate.
[0017] The antioxidant is one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester, 4-[(4,6-dioctylthio-1,3,5-triazine-2-yl)amino]-2,6-di-tert-butylphenol, propoxylated glycerol triacrylate, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol ester, tris(2,4-di-tert-butylphenyl) phosphite, (polysuccinic acid (4-hydroxy-2,2,6,6,-tetramethyl-1-piperidinylethanol) ester, and sebacic acid bis-2,2,6,6-tetramethylpiperidinol ester.
[0018] The acid scavenger is one or more of magnesium oxide, zinc oxide, aluminum oxide, magnesium hydroxide, and aluminum hydroxide.
[0019] The white filler is one or more of titanium dioxide, white carbon black and barium sulfate.
[0020] The method for preparing a co-extruded film capable of reducing hidden cracks and white overflow comprises the following steps: adding the raw materials of a white EVA film layer and the raw materials of a transparent EVA film layer into the hopper of an extruder respectively, melt co-extruding, extruding through a co-extrusion die head, cooling through an embossed casting roller, measuring thickness, shaping, trimming, and winding up, and then irradiating the surface of the white EVA film layer of the wound co-extruded film through an irradiation device and packaging and storing the film.
[0021] The co-extruded adhesive film for reducing hidden cracks and white overflow provided by the present invention is composed of a white EVA film layer and a transparent EVA film layer, wherein the white EVA film layer is pre-crosslinked by irradiation, the transparent EVA film layer is not pre-crosslinked by irradiation, and the raw material contains unsaturated carboxylic acid ester. When in use, the transparent EVA film layer contacts the photovoltaic module, so that since the transparent EVA film layer is not cross-linked, there will be no hidden crack problem during pressing, and the white EVA film layer has poor fluidity due to the high pre-crosslinking degree, and there will be no white overflow. Even if there is a small amount of white overflow, it will not overflow to the surface of the photovoltaic module due to the isolation of the transparent EVA film layer.
[0022] The co-extruded adhesive film for reducing hidden cracks and whitening provided by the present invention is obtained by melt co-extrusion molding using a conventional process method, and then irradiating the surface of a white EVA film layer with an irradiation device. In order to ensure that the white EVA film layer is irradiated to reduce fluidity, the irradiation depth is slightly greater than the thickness of the white layer adhesive film, and a part of the irradiated electrons will penetrate into the transparent EVA film layer. In order to further reduce the processing impact, the present invention adds 0.3-0.7% of the weight of an unsaturated carboxylic acid ester with a single carbon-carbon double bond to the raw material of the transparent EVA film layer. Such substances contain carbon-carbon double bonds. Part of the irradiated electrons that reach the transparent EVA film layer will attack the carbon-carbon double bonds of the unsaturated carboxylic acid ester, open the double bonds to form free radicals, and then the free radicals attack the EVA main body to form grafting. In this way, the irradiated electrons in the transparent EVA film layer are consumed without increasing the crosslinking degree, and the PID performance of the transparent EVA film layer can be enhanced to a certain extent. The residual unsaturated carboxylic acid ester will be grafted on the EVA main body by the free radical reaction provided by the crosslinking agent during component lamination, and has no effect on the reliability of the component.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The co-extruded adhesive film with reduced hidden cracking and white overflow provided by the present invention can be produced under the existing white film production equipment process, and the production process is simple; it can not only improve white overflow but also reduce the risk of hidden cracking to the level of ordinary transparent adhesive films. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the structure of the co-extruded film in the present invention, wherein 1 is a pre-crosslinked white EVA film layer, and 2 is a transparent EVA film layer. DETAILED DESCRIPTION
[0026] The present invention is described in detail below with reference to the embodiments.
[0027] In each embodiment and comparative example, the cross-linking agent is a compound of tert-butyl peroxy-2-ethylhexanoate and tert-amyl peroxy (2-ethylhexyl) carbonate in a mass ratio of 1:1; the coupling agent is γ-methacryloxypropyltrimethoxysilane, the auxiliary cross-linking agent is a compound of triallyl isocyanurate, ethoxylated trimethylolpropane triacrylate, and trimethylolpropane triacrylate in a mass ratio of 1:1:1, the antioxidant is a compound of bis-2,2,6,6-tetramethylpiperidinol sebate and β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol in a mass ratio of 1:1, the acid scavenger is magnesium oxide, and the white filler is titanium dioxide.
[0028] Example 1
[0029] A co-extruded film, the co-extruded film is composed of a white EVA film layer and a transparent EVA film layer in a thickness ratio of 3:2, and the overall weight of the film is 420g / m 2 ;
[0030] The raw material composition of the white EVA film layer and the weight proportions of each raw material are: 100 parts of EVA resin with a melt index of 15g / 10min, 1 part of a crosslinking agent, 0.4 parts of a coupling agent, 1.8 parts of a co-crosslinking agent, 0.4 parts of an antioxidant, 1.0 parts of an acid scavenger, and 8 parts of a white filler.
[0031] The raw material composition of the transparent EVA film layer and the weight proportion of each raw material are: 100 parts of EVA resin with a melt index of 25g / 10min, 0.6 parts of a crosslinking agent, 0.3 parts of a coupling agent, 1.5 parts of a co-crosslinking agent, 0.2 parts of an antioxidant, 0.1 parts of an acid scavenger, and 0.5 parts of methyl acrylate.
[0032] The preparation method of the co-extruded film is as follows: the raw materials of the white EVA film layer and the raw materials of the transparent EVA film layer are mixed evenly respectively, and then added into the extruder hopper respectively, melt co-extruded, extruded through a co-extrusion die head, cooled by an embossed casting roller, thickness measured, shaped, trimmed, and rolled up, and then the rolled co-extruded film is irradiated with an irradiation device on the surface of the white EVA film layer and then packaged and stored, the irradiation pulling speed is 20m / min, and the irradiation beam current is 35mA.
[0033] Example 2
[0034] A co-extruded film, the co-extruded film is composed of a white EVA film layer and a transparent EVA film layer in a thickness ratio of 3:2, and the overall gram weight of the film is 390g / m 2 ;
[0035] The raw material composition of the white EVA film layer and the weight proportions of each raw material are: 100 parts of EVA resin with a melt index of 15g / 10min, 1 part of a crosslinking agent, 0.4 parts of a coupling agent, 1.8 parts of a co-crosslinking agent, 0.4 parts of an antioxidant, 1.0 parts of an acid scavenger, and 8 parts of a white filler.
[0036] The raw material composition of the transparent EVA film layer and the weight proportion of each raw material are: 100 parts of EVA resin with a melt index of 25g / 10min, 0.6 parts of a crosslinking agent, 0.3 parts of a coupling agent, 1.5 parts of a co-crosslinking agent, 0.2 parts of an antioxidant, 0.1 parts of an acid scavenger, and 0.5 parts of methyl acrylate.
[0037] The preparation method of the co-extruded film is as follows: the raw materials of the white EVA film layer and the raw materials of the transparent EVA film layer are mixed evenly respectively, and then added into the extruder hopper respectively, melt co-extruded, extruded through a co-extrusion die head, cooled by an embossed casting roller, thickness measured, shaped, trimmed, and rolled up, and then the rolled co-extruded film is irradiated with an irradiation device on the surface of the white EVA film layer and then packaged and stored, the irradiation pulling speed is 20m / min, and the irradiation beam current is 38mA.
[0038] Example 3
[0039] A co-extruded film, the co-extruded film is composed of a white EVA film layer and a transparent EVA film layer in a thickness ratio of 3:2, and the overall gram weight of the film is 390g / m 2 ;
[0040] The raw material composition of the white EVA film layer and the weight proportions of each raw material are: 100 parts of EVA resin with a melt index of 15g / 10min, 1 part of a crosslinking agent, 0.4 parts of a coupling agent, 1.8 parts of a co-crosslinking agent, 0.4 parts of an antioxidant, 1.0 parts of an acid scavenger, and 8 parts of a white filler.
[0041] The raw material composition of the transparent EVA film layer and the weight proportion of each raw material are: 100 parts of EVA resin with a melt index of 25g / 10min, 0.6 parts of a crosslinking agent, 0.3 parts of a coupling agent, 1.5 parts of a co-crosslinking agent, 0.2 parts of an antioxidant, 0.1 parts of an acid scavenger, and 0.5 parts of ethyl acrylate.
[0042] The preparation method of the co-extruded film is as follows: the raw materials of the white EVA film layer and the raw materials of the transparent EVA film layer are mixed evenly respectively, and then added into the extruder hopper respectively, melt co-extruded, extruded through a co-extrusion die head, cooled by an embossed casting roller, thickness measured, shaped, trimmed, and rolled up, and then the rolled co-extruded film is irradiated with an irradiation device on the surface of the white EVA film layer and then packaged and stored, the irradiation pulling speed is 20m / min, and the irradiation beam current is 38mA.
[0043] Comparative Example 1
[0044] The same as Example 2, except that the raw material of the transparent EVA film layer does not contain methyl acrylate.
[0045] The properties of the co-extruded films prepared in the above embodiments and comparative examples are shown in Table 1.
[0046] Table 1
[0047]
[0048] The performance test methods in Table 1 are as follows:
[0049] Overall pre-crosslinking degree of the film: Use scissors to cut the film into small particles less than 3mm*3mm for later use; Cut the 120-mesh filter into 120mm*60mm, then fold it in half along the short side into 60*60mm, and fold 15mm on both sides to form an open pocket of 60*30mm; Use a balance (accuracy to 0.001g) to weigh the filter pocket and record it as W1, weigh 0.5±0.01g of the cut film particles and put them into the filter pocket, record the film weight as W2, and use copper wire to tie the filter pocket. Tighten and mark it and place it in a three-necked flask filled with xylene solution, use a heating jacket to heat the xylene, set the heating temperature to 140℃ to heat the xylene, use a condenser to cool and reflux the slightly boiling xylene, heat it at slightly boiling for 5 hours, after heating, put the filter bag with the sample into a vacuum drying oven at 140℃ and dry it for 3 hours to remove the solvent, then take out the filter bag and cool it to room temperature for 30 minutes, remove the copper wire and weigh it and record it as W3, record the pre-crosslinking degree C = ((W3-W1) / W2)*100%, measure three groups and take the average value.
[0050] Backplane peeling force: Cut the film into two pieces of 10cm*9cm, and the backplane into 3*1cm*30cm, with a width tolerance of ±0.5mm. Prepare laminated samples according to the glass / film / film / backplane stacking method (transparent EVA film layer is laminated to glass, and white EVA film layer is laminated to backplane). Laminate the above samples according to the following process: first, vacuumize at 120℃ for 320s, pressurize at -70kPa for 15s, and pressurize at -5 The pressure was maintained at 0kPa for 15s and at -30kPa for 120s. Then, at a temperature of 150°C, vacuum was drawn for 10s, pressure was applied at -70kPa for 15s, pressure was applied at -50kPa for 15s and pressure was applied at -30kPa for 430s. After the samples were laminated, they were cooled at room temperature for 2h and then tested. A tensile testing machine was used to pull the 10mm back panel off the film at 180°. The tensile force in the stable section was recorded as the back panel peeling force. The average value of the three groups was measured.
[0051] Reflectivity: Take a 12cm*9cm adhesive film, put a layer of release film on both sides. The size of the release film is larger than the size of the adhesive film. Stack them in the order of glass / release film / single-layer adhesive film / release film from bottom to top, and laminate the above samples according to the same process as the above (backplane peeling force test); take out and cool to room temperature, use a spectrophotometer to test the reflectivity of the white EVA film layer in the range of 400-700nm after lamination, take the average reflectivity in the range of 400-700nm as the reflectivity value, and measure three groups and take the average value.
[0052] Film volume resistivity: Take a film of size 100mm*100mm and stack it in the order of glass / release film / single-layer film / release film from bottom to top, laminate the above samples according to the same process as the above (backplane peeling force test), take out and cool to 25℃±2℃, use a volume resistivity meter to test the resistance for 10 minutes, and calculate the volume resistivity based on the measured sample area and thickness.
[0053] White overflow rate: When the film is laminated in the component factory, the white overflow defects generated in a single shift divided by the total production of the single shift is the white overflow rate.
[0054] Hidden crack rate: When the film is laminated in the component factory, the hidden crack defects generated in a single shift divided by the total production of the single shift is the hidden crack rate.
[0055] It can be seen from Table 1 that the co-extruded film prepared according to the scheme of the present invention will not have white overflow and hidden cracks; through the comparison of Example 2 and Comparative Example 1, it can be seen that if methyl acrylate is not used in the raw materials of the transparent EVA film layer, the co-extruded film will cause hidden cracks. This is because part of the irradiated electrons penetrate into the transparent EVA film layer during irradiation, resulting in an increase in the crosslinking degree and hardness of the transparent EVA film layer, and hidden cracks appear during component lamination.
[0056] The detailed description of a co-extruded adhesive film for reducing hidden cracks and white overflow and its preparation method with reference to the above-mentioned embodiments is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.
Claims
1. A co-extruded film for reducing hidden cracks and whitening, characterized in that: The co-extruded film consists of a white EVA film layer and a transparent EVA film layer; the white EVA film layer is pre-crosslinked by irradiation; the raw material of the transparent EVA film layer contains unsaturated carboxylic acid ester with a single carbon-carbon double bond; and the transparent EVA film layer is not crosslinked by irradiation.
2. The co-extruded film for reducing hidden cracks and whitening according to claim 1, characterized in that: In the transparent EVA film layer, the weight ratio of the unsaturated carboxylic acid ester with a single carbon-carbon double bond to the EVA resin is 0.3-0.7:
100.
3. The co-extruded film for reducing hidden cracks and whitening according to claim 1, characterized in that: The unsaturated carboxylic acid ester with a single carbon-carbon double bond is any one or more of methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, and butyl acrylate.
4. The co-extruded film for reducing hidden cracks and whitening according to any one of claims 1 to 3, characterized in that: The thickness ratio of the white EVA film layer to the transparent EVA film layer is 3:
2.
5. The co-extruded film for reducing hidden cracks and whitening according to any one of claims 1 to 3, characterized in that: When the white EVA film layer is irradiated for pre-crosslinking, the irradiation pulling speed is 15-25 m / min, and the irradiation beam current is 35-40 mA.
6. The co-extruded film for reducing hidden cracks and whitening according to any one of claims 1 to 3, characterized in that: The white EVA film layer uses EVA resin with a melt index of 3-15g / 10min as the main material.
7. The co-extruded film for reducing hidden cracks and whitening according to any one of claims 1 to 3, characterized in that: The transparent EVA film layer uses EVA resin with a melt index of 15-50g / 10min as the main material.
8. The co-extruded film for reducing hidden cracks and whitening according to any one of claims 1 to 3, characterized in that: The raw materials of the white EVA film layer are the following substances in weight: 100 parts of EVA resin with a melt index of 3-15g / 10min, 0.5-1.5 parts of a crosslinking agent, 0.2-1.0 parts of a coupling agent, 1.0-2.0 parts of a co-crosslinking agent, 0.2-1.0 parts of an antioxidant, 0.1-1.0 parts of an acid scavenger, and 5-10 parts of a white filler.
9. The co-extruded film for reducing hidden cracks and whitening according to any one of claims 1 to 3, characterized in that: The raw materials of the transparent EVA film layer are the following substances in weight: 100 parts of EVA resin with a melt index of 15-50g / 10min, 0.5-1 parts of a crosslinking agent, 0.2-0.7 parts of a coupling agent, 1.0-2.0 parts of a co-crosslinking agent, 0.2-0.5 parts of an antioxidant, 0.1-0.5 parts of an acid scavenger, and 0.3-0.7 parts of an unsaturated carboxylic acid ester with a single carbon-carbon double bond.
10. The method for preparing a co-extruded film with reduced hidden cracks and whitening according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: adding raw materials of a white EVA film layer and a transparent EVA film layer into an extruder hopper respectively, melt co-extruding, extruding through a co-extrusion die head, cooling through an embossed casting roller, measuring thickness, shaping, trimming, and rolling up, and then irradiating the surface of the white EVA film layer with an irradiation device and packaging the rolled co-extruded film for storage.