Spoke type non-pneumatic tire and preparation method thereof

By using the adhesives of components A and components B in the spoke non-pneumatic tires, a chemical crosslinking structure between rubber and adhesive is formed, which solves the problem of insufficient bonding strength of traditional adhesives and improves the tires Adhesive performance at high speed and emergency stop conditions.

CN118995083AActive Publication Date: 2024-11-22QINGDAO LANDAU WHEEL & TRACK TECH CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411106165.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The adhesive bonding strength of traditional spoke non-pneumatic tires is low and cannot meet the adhesive bonding strength requirements during high-speed operation, emergency stop or emergency acceleration.

Method used

The adhesive of component A and component B is used to form a mesh structure through the reaction of crosslinking agent and isocyanate groups, so as to achieve chemical bonding between rubber and adhesive and improve bonding strength.

Benefits of technology

The bonding strength of the spoke-type non-pneumatic tires during high-speed operation and emergency stop or emergency acceleration is improved, ensuring good bonding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995083A_ABST
    Figure CN118995083A_ABST
Patent Text Reader

Abstract

The invention provides a spoke type non-pneumatic tire and a preparation method thereof, and relates to the technical field of tires, the spoke type non-pneumatic tire at least comprises a wheel face and a bonding layer, the bonding layer is located on one side of the wheel face and used for being bonded with the wheel face, the bonding layer comprises a bonding agent, the wheel face comprises primer rubber, and the bonding agent is used for being crosslinked with the primer rubber; the adhesive comprises a component A and a component B, and the ratio range of the component A to the component B is (100: 30)-(100: 80); the component A comprises the following components in parts by weight: 80-100 parts of olefin rubber; 3-6 parts of an anti-aging agent; 1-3 parts of an accelerant; 1-3 parts of a cross-linking agent; 3-10 parts of an activating agent; 40 to 60 parts of a reinforcing agent; 60 to 200 parts of a solvent A; the component B comprises the following components in parts by weight: 30-60 parts of epoxy resin; 5 to 30 parts of isocyanate; 1-3 parts of fatty amine; 60 to 100 parts of polyhydric alcohol; and 60-100 parts of a solvent B. Therefore, the requirement of the spoke type non-pneumatic tire on the bonding strength of the adhesive during sudden stop or rapid acceleration in the high-speed running process can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of tire technology, and in particular to a spoke-type non-pneumatic tire and a preparation method thereof. Background Art

[0002] With the development of technology, spoke-type non-pneumatic tires, as tires for the new generation of electric vehicles, have been increasingly widely studied and applied. Spoke-type non-pneumatic tires usually consist of three parts: the wheel surface, the spokes, and the hub. The way these three parts are fitted together will affect the performance of the entire spoke-type non-pneumatic tire.

[0003] The spokes and the wheel surface of the spoke-type non-pneumatic tire are usually bonded together using an adhesive layer. The rubber constituting the wheel surface is mostly natural rubber, styrene-butadiene rubber, butadiene rubber and isoprene rubber, etc. These rubbers are non-polar, and the adhesive commonly used at present has low bonding strength after bonding the spokes and the wheel surface, which cannot meet the bonding strength requirements of the spoke-type non-pneumatic tire during high-speed operation, sudden stop or sudden acceleration.

[0004] Therefore, it is urgent to develop a new adhesive for spoke-type non-pneumatic tires to solve the above problems. Summary of the invention

[0005] The embodiments of the present application provide a spoke-type non-pneumatic tire and a preparation method thereof, thereby solving the problem that the adhesive used in the adhesive layer of a conventional spoke-type non-pneumatic tire has low bonding strength, resulting in the inability to meet the bonding strength requirements of the adhesive during high-speed operation, sudden stop or sudden acceleration of the spoke-type non-pneumatic tire.

[0006] To achieve the above objectives, the embodiments of the present application adopt the following technical solutions:

[0007] On the one hand, a spoke-type non-pneumatic tire is provided, the spoke-type non-pneumatic tire at least comprising a wheel surface and an adhesive layer, the adhesive layer is located on one side of the wheel surface and is used to be bonded to the wheel surface, the adhesive layer comprises an adhesive, the wheel surface comprises a base rubber, and the adhesive is used to cross-link with the base rubber;

[0008] The adhesive comprises component A and component B, and the ratio of component A to component B is in the range of 100:30-100:80;

[0009] The A component comprises by weight:

[0010] Olefin rubber, 80-100 parts;

[0011] Anti-aging agent, 3-6 parts;

[0012] Accelerator, 1-3 parts;

[0013] Cross-linking agent, 1-3 parts;

[0014] Activator, 3-10 parts;

[0015] Reinforcing agent, 40-60 parts;

[0016] A solvent, 60-200 parts;

[0017] The B component comprises by weight:

[0018] Epoxy resin, 30-60 parts;

[0019] Isocyanate, 5-30 parts;

[0020] Fatty amine, 1-3 parts;

[0021] Polyol, 60-100 parts;

[0022] B solvent, 60-100 parts.

[0023] Further, the peel strength of the adhesive layer is in the range of 23-33 KN / m. Further, the antioxidant comprises a secondary amine antioxidant;

[0024] The accelerator includes a sulfenamide accelerator;

[0025] The cross-linking agent includes sulfur;

[0026] The activator includes a metal inorganic activator;

[0027] The reinforcing agent includes carbon black;

[0028] The solvent A includes at least one of ketones and aromatic hydrocarbons. Further, the epoxy resin includes bisphenol A epoxy resin;

[0029] The isocyanate includes diisocyanate;

[0030] The fatty amine includes a fatty amine having a double active group;

[0031] The polyols include polyols containing both olefin bonds and multiple hydroxyl groups.

[0032] The B solvent includes at least one of ketones and aromatic hydrocarbons.

[0033] Furthermore, the base rubber of the wheel tread includes natural rubber.

[0034] Furthermore, the spoke-type non-pneumatic tire further comprises a spoke, wherein the spoke is located on a side of the adhesive layer away from the wheel surface, and the adhesive layer is also used to bond with the spoke;

[0035] The material of the spokes includes any one of polyurethane and modified polyurethane.

[0036] On the other hand, a method for preparing the spoke-type non-pneumatic tire as described above is provided, comprising the following steps:

[0037] Cleaning the wheel surface of the spoke-type non-pneumatic tire;

[0038] preparing the adhesive;

[0039] Applying the adhesive to one side surface of the wheel surface;

[0040] Laminating the wheel surface coated with the adhesive to the wheel spokes to form the spoke-type non-pneumatic tire preparation;

[0041] The spoke-type non-pneumatic tire preform is injection molded to obtain the spoke-type non-pneumatic tire; wherein the injection molding temperature ranges from 130 to 260° C., the insulation time ranges from 1 to 30 minutes after injection molding, the injection molding pressure ranges from 40 to 80 MPa, and the injection mold temperature ranges from 30 to 130° C.

[0042] Further, the preparation of the adhesive comprises:

[0043] Producing the A component;

[0044] Producing the B component;

[0045] The component A and the component B are uniformly mixed in a ratio of 100:30-100:80 to obtain the adhesive.

[0046] Further, the preparation of the A component comprises:

[0047] The olefin rubber is kneaded at 50-60° C. for a period of time, then heated to 80-90° C., the antioxidant, the accelerator, the activator and the reinforcing agent are added, and the kneading is continued and the temperature is raised to 150-160° C., and the rubber is discharged to obtain a first rubber compound;

[0048] The first rubber material is kept at 20-25° C. for a period of time, then heated to 50-60° C., the cross-linking agent is added and the rubber material is kneaded for a period of time, and then heated to 90-100° C. to produce the rubber material, thereby obtaining the second rubber material.

[0049] The second rubber material and the A solvent are uniformly mixed to obtain the A component.

[0050] Further, the preparation of the B component comprises:

[0051] Dehydrating the epoxy resin at 110-120° C. to obtain a dehydrated epoxy resin;

[0052] After cooling the dehydrated epoxy resin to 50-60° C., adding the fatty amine to obtain a modified epoxy resin;

[0053] After cooling the modified epoxy resin to 20-30° C., adding the solvent B and mixing evenly to obtain a uniform solution;

[0054] Dehydrating the polyol at 110-120° C. to obtain a dehydrated polyol;

[0055] After cooling the dehydrated polyol to 50-60° C., adding the isocyanate to obtain a mixture containing an isocyanate group at the end and an isocyanate;

[0056] The mixture containing isocyanate groups at the ends and isocyanate is mixed evenly with the uniform solution, and reacted at 30-40° C. for a period of time to obtain the B component.

[0057] The embodiments of the present application provide a spoke-type non-pneumatic tire and a preparation method thereof. Through the molecular structure design of the adhesive itself, a polyurethane-modified epoxy resin containing double bonds can be co-vulcanized with the rubber wheel surface or the rubber in component A to form a network structure, so that the adhesive and the rubber wheel surface are combined by chemical bonds to form a chemically cross-linked structure as a whole. The resulting bonding strength is high and the bonding performance is good. Therefore, the bonding strength requirements of the spoke-type non-pneumatic tire during high-speed operation, sudden stop or sudden acceleration can be met.

[0058] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0060] Figure 1 A schematic structural diagram of a spoke-type non-pneumatic tire provided in an embodiment of the present application;

[0061] Figure 2A schematic diagram of bonding an adhesive to a rubber wheel surface provided in an embodiment of the present application;

[0062] Figure 3 A process flow chart of a spoke-type non-pneumatic tire according to an embodiment of the present application;

[0063] Figure 4 A process flow chart of a preparation process of an adhesive provided in an embodiment of the present application;

[0064] Figure 5 A process flow chart of another adhesive preparation method provided in an embodiment of the present application;

[0065] Figure 6 A flow chart of a preparation process of another adhesive provided in an embodiment of the present application. DETAILED DESCRIPTION

[0066] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0067] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0068] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or multiple, respectively.

[0069] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0070] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0071] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0072] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0073] In a first aspect, an embodiment of the present application provides a spoke-type non-pneumatic tire, which comprises at least a wheel tread and an adhesive layer, wherein the adhesive layer is located on one side of the wheel tread and is used to bond with the wheel tread, the adhesive layer comprises an adhesive, the wheel tread comprises a base rubber, the adhesive is used to cross-link with the base rubber, the adhesive comprises a component A and a component B, and the ratio of the component A to the component B is in the range of 100:30-100:80.

[0074] Among them, component A includes, by weight: olefin rubber, 80-100 parts; antioxidant, 3-6 parts; accelerator, 1-3 parts; crosslinking agent, 1-3 parts; activator, 3-10 parts; reinforcing agent, 40-60 parts; A solvent, 60-200 parts.

[0075] The B component comprises, by weight: 30-60 parts of epoxy resin; 5-30 parts of isocyanate; 1-3 parts of fatty amine; 60-100 parts of polyol; and 60-100 parts of B solvent.

[0076] In practical applications, when the ratio of component A to component B is too high or too low, the strength of the adhesive is too low. Therefore, the ratio of component A to component B can be set in the range of 100:30-100:80, so that the strength of the adhesive can be better. Exemplarily, the ratio of component A to component B can be 100:30, 100:40, 100:50, 100:60, 100:70 or 100:80, etc.

[0077] It should be understood that the above-mentioned spoke-type non-pneumatic tire at least includes a wheel surface and an adhesive layer. Figure 1 As shown, the spoke-type non-pneumatic tire includes a wheel surface and an adhesive layer, a wheel spoke and a wheel hub, the wheel spoke is located on the side of the adhesive layer away from the wheel surface, and the wheel spoke includes a plurality of spokes, one end of each spoke is used to be connected to the wheel surface after being bonded by the adhesive layer, and the other end of each spoke is connected to the wheel hub. Of course, the spoke-type non-pneumatic tire also has other structures, and only the contents related to the invention are described here, and other contents can be obtained through related technologies.

[0078] In practical applications, the olefin rubber in component A refers to a rubber containing double bonds in the molecular chain, for example, cis-1,4-polybutadiene rubber (cis-butadiene rubber for short), etc. For example, the olefin rubber can be 80 parts, 85 parts, 90 parts, 95 parts, 98 parts or 100 parts by weight.

[0079] The antioxidant can be a secondary amine antioxidant, which can be used as a stabilizer and has good protective effect against aging caused by light, heat, ozone, etc. during the synthesis process. The secondary amine antioxidant can include RD445, etc., which is a low-pollution aromatic secondary amine antioxidant with good antioxidant performance. Exemplarily, the antioxidant can be 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts or 6 parts by weight.

[0080] The above-mentioned accelerator can be a sulfonamide accelerator. Sulfonamide accelerators are benzothiazole sulfonamide compounds used as vulcanization accelerators, which can accelerate the chemical reaction rate and promote the curing or physical properties of the cured product during the adhesive processing process. Sulfonamide accelerators can include N-cyclohexyl-2-benzothiazole sulfonamide (CZ), N-tert-butyl-2-benzothiazole sulfonamide (NS), N, N-2 dicyclohexyl-2,2-dibenzothiazole sulfonamide (DZ), N-oxydiethylene-2-benzothiazole sulfonamide (NOBS), etc. Exemplarily, the accelerator can be 1 part, 1.5 parts, 2 parts, 2.5 parts, 2.8 parts or 3 parts by weight, etc.

[0081] The cross-linking agent may be sulfur, which is also a vulcanizing agent. For example, the cross-linking agent may be 1 part, 1.5 parts, 2 parts, 2.5 parts, 2.8 parts or 3 parts by weight.

[0082] The activator can be a metal inorganic activator, for example, zinc oxide (ZnO). The activator can be used to promote the vulcanization reaction, and can also promote the blending and dispersion of the filler. The vulcanization reaction can be significantly improved by using a small amount of the activator. Exemplarily, the activator can be 3 parts, 4 parts, 5 parts, 6 parts, 7 parts or 10 parts by weight.

[0083] The reinforcing agent may be carbon black, etc. The activity of the surface of carbon black particles is not uniform, and there are a few strong active points and a large number of adsorption points with different energies. Therefore, carbon black has different binding energies to the rubber chains on its surface, which may be mostly adsorption caused by van der Waals forces and a few chemical bonds. Exemplarily, the reinforcing agent may be 40 parts, 45 parts, 50 parts, 55 parts, 58 parts or 60 parts by weight.

[0084] The above-mentioned solvent A can be at least one of ketones and aromatic hydrocarbons, for example, butanone, acetone, toluene and xylene, etc. Exemplarily, the solvent A can be 60 parts, 80 parts, 10 parts, 140 parts, 190 parts or 200 parts by weight.

[0085] Thus, the final component A is a compound rubber containing olefin bonds and sulfur, and is dissolved in the A solvent.

[0086] In practical applications, the epoxy resin in component B may be a bisphenol A epoxy resin, such as E51, etc. For example, the epoxy resin may be 30 parts, 35 parts, 40 parts, 45 parts, 50 parts or 60 parts by weight.

[0087] The isocyanate may be a diisocyanate, for example, liquefied diphenylmethane diisocyanate (liquefied MDI), toluene diisocyanate, 1,5-naphthalene diisocyanate, etc. For example, the epoxy resin may be 5 parts, 8 parts, 10 parts, 15 parts, 20 parts, or 30 parts by weight.

[0088] The above-mentioned fatty amine can be a fatty amine having a dual active group, for example, diethylenetriamine, etc. Exemplarily, the fatty amine can be 1 part, 1.5 parts, 2 parts, 2.5 parts, 2.8 parts or 3 parts by weight.

[0089] The polyol may be a molecule containing both an olefin bond and a hydroxyl group, and the number of hydroxyl groups is greater than or equal to 2, for example, hydroxy-terminated polybutadiene, etc. For example, the polyol may be 60 parts, 70 parts, 80 parts, 85 parts, 90 parts or 100 parts by weight.

[0090] The above-mentioned solvent B can be at least one of ketones and aromatic hydrocarbons, for example, butanone, acetone, toluene and xylene, etc. Exemplarily, the solvent B can be 60 parts, 70 parts, 80 parts, 85 parts, 90 parts or 100 parts by weight.

[0091] Therefore, since component B is a modified product containing isocyanate at the end, its modified epoxy resin and polyol will have two reactions in the following: 1. After modification, the molecules of component B contain both double bonds and isocyanate groups, and the double bonds can further cross-link the sulfur of component A with the base rubber to the molecules of the base rubber; and 2. The isocyanate in component B can react with the polyol to form polyurethane through condensation reaction, and the polyurethane can modify the epoxy resin to make component B a modified epoxy resin, and at the same time introduce double bonds, amide groups and amino groups into its molecules, so the isocyanate groups of component B can further react with the amide groups on the polyurethane molecules to achieve chemical linkage between the two molecules.

[0092] In summary, the adhesive of the embodiment of the present application can be synthesized by component A and component B, and the peel strength of the adhesive ranges from 23 to 33 KN / m. Exemplarily, the peel strength of the adhesive can be 23 KN / m, 25 KN / m, 28 KN / m, 29 KN / m, 30 KN / m or 33 KN / m, etc.

[0093] In practical applications, the base rubber of the wheel surface may include natural rubber. Conventional natural rubber may use any natural rubber as long as it is known as natural rubber, and the origin is not limited. For example, natural rubber may contain cis-1,4-polyisoprene as the main agent, and may also contain trans-1,4-polyisoprene according to the required properties. Therefore, in addition to the natural rubber containing cis-1,4-polyisoprene as the main agent, the natural rubber may also contain trans-1,4-isoprene as the main agent.

[0094] Thus, during the process of applying the adhesive prepared in the embodiment of the present application to the base rubber of the wheel surface and curing, the adhesive can be bonded to the base rubber in the following manner: Figure 2 shown.

[0095] The embodiment of the present application provides an adhesive, which, through the design of the molecular structure of the adhesive itself, allows the polyurethane-modified epoxy resin containing double bonds to be co-vulcanized with the rubber wheel surface or the rubber in component A to form a network structure, so that the adhesive and the rubber wheel surface are combined by chemical bonds to form a chemically cross-linked structure as a whole, and the resulting bonding strength is high and the bonding performance is good. Therefore, it can meet the bonding strength requirements of the spoke-type non-pneumatic tire during high-speed operation, sudden stop or sudden acceleration.

[0096] Furthermore, the material of the spokes includes any one of polyurethane and modified polyurethane.

[0097] It should be noted that the main molding process of the spoke-type non-pneumatic tire is to vulcanize the wheel surface, perform surface treatment on the hub, and then perform injection molding on the spokes. The spokes and the wheel surface are bonded by an adhesive layer formed by an adhesive.

[0098] The embodiment of the present application provides an adhesive. Through the design of the molecular structure of the adhesive itself, a polyurethane-modified epoxy resin containing double bonds can be co-vulcanized with the rubber wheel surface or the rubber in component A to form a network structure. At the same time, the isocyanate group can react with the carbamate group in the spoke to form a covalent bond, that is, covalently bonded to its molecule. In this way, the spoke, the adhesive, and the rubber wheel surface can be combined by chemical bonds to form a chemically cross-linked structure as a whole, thereby obtaining a higher bonding strength and good bonding performance. Therefore, the bonding strength requirements of the spoke-type non-pneumatic tire during high-speed operation, sudden stop or sudden acceleration of the adhesive can be met.

[0099] In a second aspect, an embodiment of the present application provides a method for preparing the above-mentioned spoke-type non-pneumatic tire.

[0100] like Figure 3 As shown, the preparation method of the spoke-type non-pneumatic tire comprises the following steps:

[0101] S1. Clean the wheel surface of the spoke-type non-pneumatic tire.

[0102] S2. Prepare an adhesive.

[0103] S3. Apply adhesive to one side surface of the wheel surface.

[0104] S4. Adhere the wheel surface coated with the adhesive to the wheel spokes to form a spoke-type non-pneumatic tire preparation.

[0105] S5. Injection-molding the spoke-type non-pneumatic tire preform to obtain a spoke-type non-pneumatic tire.

[0106] Among them, the injection temperature range is 130-260°C, the insulation time range after injection molding is 1-30min, the injection pressure range is 40-80MPa, and the injection mold temperature range is 30-130°C.

[0107] It should be noted that there is no specific limitation on the order of the above steps S1 and S2. Step S1 may be performed first and then step S2, or step S2 may be performed first and then step S1, or step S1 and step S2 may be performed simultaneously.

[0108] In practical applications, the spoke-type non-pneumatic tire preparation may be injection molded in an injection molding machine.

[0109] Exemplarily, the injection molding temperature can be 130°C, 160°C, 200°C, 220°C, 240°C or 260°C, etc., the holding time after injection molding can be 1 min, 5 min, 10 min, 15 min, 20 min or 30 min, etc., the injection molding pressure can be 40 MPa, 50 MPa, 60 MPa, 65 MPa, 60 MPa or 80 MPa, etc., and the injection mold temperature can be 30°C, 40°C, 50°C, 80°C, 100°C or 130°C, etc.

[0110] The injection molding process can promote the co-vulcanization reaction between the adhesive and the rubber wheel surface, so that the rubber part of the adhesive and the rubber wheel surface can be chemically linked to each other through the molecular chain; and the isocyanate-modified epoxy resin containing double bonds can be co-vulcanized with the rubber wheel surface or the rubber in component A to form a network structure. At the same time, the isocyanate group can react with the carbamate group in the spoke to form a covalent bond, that is, covalently bond with its molecules, so that the spoke, adhesive and rubber wheel surface are combined by chemical bonds, ensuring good bonding strength, thereby meeting the bonding strength requirements of the spoke-type non-pneumatic tire during high-speed operation, sudden stop or sudden acceleration.

[0111] Furthermore, if Figure 4 As shown, the above step S2. of preparing the adhesive comprises:

[0112] S21. Prepare component A.

[0113] S22. Prepare component B.

[0114] S23. Component A and component B are uniformly mixed in a ratio of 100:30-100:80 to obtain an adhesive.

[0115] Furthermore, if Figure 5 As shown, the above step S21. preparing component A comprises:

[0116] S211. After kneading the olefin rubber at 50-60°C for a period of time, the temperature is raised to 80-90°C, an antioxidant, a accelerator, an activator and a reinforcing agent are added, the kneading is continued and the temperature is raised to 150-160°C, and the rubber is discharged to obtain the first rubber compound.

[0117] In practical applications, olefin rubber can be placed in an internal mixer for internal mixing. Internal mixing is to mix the raw rubber with various auxiliary materials together.

[0118] It should be understood that the above-mentioned internal mixing of the olefin rubber at 50-60° C. can reduce the difficulty of subsequent plasticizing.

[0119] The above-mentioned heating to 80-90°C is to break up the raw rubber.

[0120] The above-mentioned temperature increase to 150-160° C. is for mixing.

[0121] S212. After the first rubber compound is kept at 20-25°C for a period of time, the temperature is raised to 50-60°C, a cross-linking agent is added and the mixture is milled for a period of time, and the temperature is raised to 90-100°C to produce the rubber compound, thereby obtaining the second rubber compound.

[0122] In practical applications, the first rubber compound can be placed in an open mill for open mixing. Open mixing is to add the rubber compound after internal mixing to the vulcanizer for further mixing in preparation for compression molding vulcanization.

[0123] It should be understood that the purpose of keeping the first rubber material at 20-25° C. for a period of time is to allow the additive to disperse better.

[0124] The above temperature rise to 90-100°C is because at this temperature, the basic rubber material mixing is completed.

[0125] S213. The second rubber material is mixed evenly with the A solvent to obtain component A.

[0126] In practical applications, the second rubber material is placed in a reaction kettle and mixed with solvent A. The purpose of mixing with solvent A is to form a uniform solution, which is convenient for subsequent mixing, dispersion, coating, and infiltration.

[0127] Furthermore, if Figure 6 As shown, the above step S22. preparing component B comprises:

[0128] S221. Dehydrate the epoxy resin at 110-120°C to obtain a dehydrated epoxy resin.

[0129] Since water reacts with isocyanate very quickly, in order to avoid consuming the groups involved in the reaction and ensure the strength of the final bonding layer, the epoxy resin is dehydrated in advance, and high-temperature dehydration is used to prevent solvent volatilization.

[0130] S222. After cooling the dehydrated epoxy resin to 50-60°C, add fatty amine to obtain modified epoxy resin.

[0131] It should be understood that the above-mentioned cooling to 50-60° C. is to prevent the subsequent reaction process from causing explosion due to excessive temperature and to promote the reaction.

[0132] S223. After cooling the modified epoxy resin to 20-30°C, add solvent B and mix evenly to obtain a uniform solution.

[0133] S224. Dehydrating the polyol at 110-120° C. to obtain a dehydrated polyol.

[0134] Since water reacts with isocyanate very quickly, in order to avoid consuming the groups involved in the reaction and ensure the strength of the final bonding layer, the polyol is dehydrated in advance, and high-temperature dehydration is used to prevent solvent volatilization.

[0135] S225. After cooling the dehydrated polyol to 50-60° C., isocyanate is added to obtain a mixture containing an isocyanate group at the end and an isocyanate group.

[0136] S226. The mixture containing isocyanate groups at the end and isocyanate is mixed evenly with the uniform solution, and reacted at 30-40° C. for a period of time to obtain component B.

[0137] It should be noted that there is no specific limitation on the order of the above steps S221-223 and steps S224-225. Steps S221-223 may be performed first and then steps S224-225, or steps S224-225 may be performed first and then steps S221-223, or steps S221-223 and steps S224-225 may be performed simultaneously.

[0138] The following is a specific preparation process of a spoke-type non-pneumatic tire:

[0139] 1. Preparation of component A:

[0140] (1) Heat the internal mixer to 50-60°C, add olefin rubber for internal mixing, heat to 80-90°C, add antioxidant, accelerator, activator and reinforcing agent, continue internal mixing and heat to 150-160°C, discharge the rubber, and obtain the first rubber compound.

[0141] (2) After the first rubber material is left at 20-25°C for 8-10 hours, it is further mixed in an open mill.

[0142] (3) Heat the mixing mill to 50-60°C, add the first rubber compound and the cross-linking agent for mixing, heat to 90-100°C, discharge the rubber, and place it at room temperature for 8-10 hours to obtain the second rubber compound.

[0143] (4) In a reaction kettle, mix the second rubber material and solvent A until they are uniform to obtain component A.

[0144] 2. Preparation of component B:

[0145] (1) Dehydrate the epoxy resin at 110-120°C, -0.1MPa, and a rotation speed of 80-100r / min for 2h, cool it to 50-60°C, add fatty amine to obtain a modified epoxy resin, then cool it to 20-30°C, add solvent B and mix to obtain a uniform solution.

[0146] (2) The polyol is dehydrated at 110-120°C, -0.1MPa, and a rotation speed of 80-100r / min for 2h. After cooling to 50-60°C, isocyanate is added to obtain a mixture containing terminal isocyanate groups and isocyanate. The mixture is mixed with the components in (1) and reacted at 30-40°C for 60min to obtain a uniform solution, i.e., component B.

[0147] 3. Mixing of component A and component B:

[0148] (1) Component A and component B are mixed at a ratio of 100:30-100:80 at 50-70 r / min until uniform, to prepare an adhesive.

[0149] 4. Combination of adhesive, wheel surface and spokes:

[0150] (1) Surface cleaning: Use a lint-free cloth to soak in dichloromethane (CH 2 Cl 2 ), wipe the rubber surface to be bonded, leave it for 5 minutes and then blow the surface clean with compressed air.

[0151] (2) Coating: Use coating equipment to apply the adhesive to the rubber surface. The number of coatings is 1-2 times, and the dry film thickness is 10-35μm.

[0152] (3) Pretreatment: Place the coated sample at ambient temperature or in a constant temperature device at 15-35℃ for more than 30 minutes, and then bond after the surface is dry.

[0153] (4) Bonding: The rubber surface coated with the adhesive is bonded to the wheel spokes and maintained at a pressure of 0.5-5 MPa and a temperature of 40-170°C for 3-25 minutes.

[0154] (5) Finished product: Place the bonded product at 80-120°C for 10-20 minutes to obtain the finished product.

[0155] (6) Injection molding process: The finished product is injection molded in an injection molding machine.

[0156] It should be noted that the description of the olefin rubber, antioxidant, accelerator, cross-linking agent, activator, reinforcing agent, solvent A, epoxy resin, fatty amine, polyol, isocyanate and solvent B in the embodiments of the present application can be referred to the above embodiments and will not be repeated here.

[0157] The adhesive / spoke type non-pneumatic tire of the present application and the comparative example and the preparation method and application thereof are illustrated by multiple specific embodiments below.

[0158] Example 1

[0159] (1) Heat the internal mixer to 50°C, add natural rubber for internal mixing, heat to 80°C, add antioxidant, accelerator, activator and reinforcing agent, continue internal mixing and heat to 155°C, discharge the rubber, and obtain the first rubber compound.

[0160] (2) After the first rubber compound is left at 20-22°C for 8 hours, it is further mixed in an open mill.

[0161] (3) Heat the mixer to 55°C, add the first rubber compound and the cross-linking agent and start mixing. Heat the mixer to 95°C, discharge the rubber compound, and place it at room temperature for 8 hours to obtain the second rubber compound.

[0162] (4) In a reaction kettle, mix the second rubber material and solvent A until they are uniform to obtain component A.

[0163] (5) The epoxy resin was dehydrated for 2 h at 120°C, -0.1 MPa, and a rotation speed of 80 r / min. After cooling to 50°C, a fatty amine was added to obtain a modified epoxy resin. The mixture was then cooled to 25°C and solvent B was added and mixed to obtain a uniform solution.

[0164] (6) The polyol was dehydrated at 120°C, -0.1MPa, and a rotation speed of 80r / min for 2h. After cooling to 50°C, isocyanate was added to obtain a mixture containing terminal isocyanate groups and isocyanate. The mixture was mixed with the components in (1) and reacted at 30°C for 60min to obtain a uniform solution, i.e., component B.

[0165] (7) Component A and component B were mixed at 70 r / min at a ratio of 100:30 until they were uniform, to prepare an adhesive.

[0166] (8) Injection molding process: The rubber surface coated with the adhesive is bonded to the spoke to obtain a finished product, and the finished product is maintained in an injection molding machine at 70°C and 4 MPa for 15 minutes.

[0167] Example 2

[0168] (1) Heat the internal mixer to 55°C, add natural rubber for internal mixing, heat to 90°C, add antioxidant, accelerator, activator and reinforcing agent, continue internal mixing and heat to 155°C, discharge the rubber, and obtain the first rubber compound.

[0169] (2) After the first rubber compound is left at 22°C for 8 hours, it is further mixed in an open mill.

[0170] (3) Heat the mixing mill to 60°C, add the first rubber compound and the cross-linking agent for mixing, heat to 95°C, discharge the rubber, and place it at room temperature for 10 hours to obtain the second rubber compound.

[0171] (4) In a reaction kettle, mix the second rubber material and solvent A until they are uniform to obtain component A.

[0172] (5) The epoxy resin was dehydrated for 2 h at 110°C, -0.1 MPa, and a rotation speed of 80 r / min. After cooling to 55°C, a fatty amine was added to obtain a modified epoxy resin. The epoxy resin was then cooled to 25°C and solvent B was added and mixed to obtain a uniform solution.

[0173] (6) The polyol was dehydrated at 110°C, -0.1MPa, and a rotation speed of 80r / min for 2h. After cooling to 55°C, isocyanate was added to obtain a mixture containing terminal isocyanate groups and isocyanate. The mixture was mixed with the components in (1) and reacted at 33°C for 60min to obtain a uniform solution, i.e., component B.

[0174] (7) Component A and component B were mixed at 70 r / min at a ratio of 100:30 until they were uniform, to prepare an adhesive.

[0175] (8) Injection molding process: The rubber surface coated with the adhesive is bonded to the wheel spoke to obtain a finished product, and the finished product is maintained in an injection molding machine at 40°C and 5 MPa for 25 minutes.

[0176] Example 3

[0177] (1) Heat the internal mixer to 60°C, add natural rubber for internal mixing, heat to 90°C, add antioxidant, accelerator, activator and reinforcing agent, continue internal mixing and heat to 155°C, discharge the rubber, and obtain the first rubber compound.

[0178] (2) After the first rubber compound is left at 25°C for 10 hours, it is further mixed in an open mixer.

[0179] (3) Heat the mixing mill to 60°C, add the first rubber compound and the cross-linking agent for mixing, heat to 100°C, discharge the rubber, and place it at room temperature for 10 hours to obtain the second rubber compound.

[0180] (4) In a reaction kettle, mix the second rubber material and solvent A until they are uniform to obtain component A.

[0181] (5) The epoxy resin was dehydrated at 100°C, -0.1MPa, and a rotation speed of 100r / min for 2h. After cooling to 60°C, a fatty amine was added to obtain a modified epoxy resin. The epoxy resin was then cooled to 30°C and solvent B was added and mixed to obtain a uniform solution.

[0182] (6) The polyol is dehydrated at 100°C, -0.1MPa, and a rotation speed of 100r / min for 2h. After cooling to 60°C, isocyanate is added to obtain a mixture containing terminal isocyanate groups and isocyanate. The mixture is mixed with the components in (1) and reacted at 35°C for 60min to obtain a uniform solution, i.e., component B.

[0183] (7) Mix component A and component B at 50 r / min until they are uniform to obtain an adhesive.

[0184] (8) Injection molding process: The rubber surface coated with the adhesive is bonded to the wheel spoke to obtain a finished product, and the finished product is maintained at 170°C and 2 MPa for 3 minutes in an injection molding machine.

[0185] Comparative Example 1

[0186] Commercially available polyurethane was used as the adhesive.

[0187] The spoke-type non-pneumatic tires obtained in Examples 1-3 and Comparative Example 1 were tested for peel strength, and the results are shown in Table 1 below.

[0188] Among other things, the peel strength test was performed according to standard ISO 814:2007.

[0189] Table 1

[0190]

[0191] It can be seen from Table 1 that, compared with Comparative Example 1, the peel strengths of Examples 1-3 under different injection molding conditions are greater, and the bonding strength of the adhesive in the spoke-type non-pneumatic tires prepared in Examples 1-3 is very good.

[0192] This application only introduces the contents related to the invention. The remaining structures can be obtained by referring to the relevant technologies and will not be described in detail here.

[0193] An “embodiment” referred to herein means that a particular feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment of the present application.

[0194] In the description provided herein, a large number of specific details are described. However, it is understood that the embodiments of the present application can be practiced without these specific details. In some instances, well-known methods, structures and techniques are not shown in detail so as not to obscure the understanding of this description.

[0195] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A spoke-type non-pneumatic tire, characterized in that: The spoke-type non-pneumatic tire at least comprises a wheel surface and an adhesive layer, wherein the adhesive layer is located on one side of the wheel surface and is used to be bonded to the wheel surface, the adhesive layer comprises an adhesive, the wheel surface comprises a base rubber, and the adhesive is used to be cross-linked with the base rubber; The adhesive comprises component A and component B, and the ratio of component A to component B is in the range of 100:30-100:80; The A component comprises by weight: Olefin rubber, 80-100 parts; Anti-aging agent, 3-6 parts; Accelerator, 1-3 parts; Cross-linking agent, 1-3 parts; Activator, 3-10 parts; Reinforcing agent, 40-60 parts; A solvent, 60-200 parts; The B component comprises by weight: Epoxy resin, 30-60 parts; Isocyanate, 5-30 parts; Fatty amine, 1-3 parts; Polyol, 60-100 parts; B solvent, 60-100 parts.

2. The spoke-type non-pneumatic tire according to claim 1, characterized in that: The peel strength of the adhesive layer is in the range of 23-33 KN / m.

3. The spoke-type non-pneumatic tire according to claim 1 or 2, characterized in that: The antioxidant includes a secondary amine antioxidant; The accelerator includes a sulfenamide accelerator; The cross-linking agent includes sulfur; The activator includes a metal inorganic activator; The reinforcing agent includes carbon black; The A solvent includes at least one of ketones and aromatic hydrocarbons.

4. The spoke-type non-pneumatic tire according to claim 1 or 2, characterized in that: The epoxy resin includes bisphenol A type epoxy resin; The isocyanate includes diisocyanate; The fatty amine includes a fatty amine having a double active group; The polyols include polyols containing both olefin bonds and multiple hydroxyl groups. The B solvent includes at least one of ketones and aromatic hydrocarbons.

5. The spoke-type non-pneumatic tire according to claim 1 or 2, characterized in that: The base rubber of the wheel tread includes natural rubber.

6. The spoke-type non-pneumatic tire according to claim 1 or 2, characterized in that: The spoke-type non-pneumatic tire further comprises a spoke, wherein the spoke is located on a side of the adhesive layer away from the wheel surface, and the adhesive layer is also used to bond with the spoke; The material of the spokes includes any one of polyurethane and modified polyurethane.

7. A method for preparing a spoke-type non-pneumatic tire according to any one of claims 1 to 6, characterized in that: The steps include: Cleaning the wheel surface of the spoke-type non-pneumatic tire; preparing the adhesive; Applying the adhesive to one side surface of the wheel surface; Laminating the wheel surface coated with the adhesive to the wheel spokes to form the spoke-type non-pneumatic tire preparation; The spoke-type non-pneumatic tire preform is injection molded to obtain the spoke-type non-pneumatic tire; wherein the injection molding temperature ranges from 130 to 260° C., the insulation time ranges from 1 to 30 minutes after injection molding, the injection molding pressure ranges from 40 to 80 MPa, and the injection mold temperature ranges from 30 to 130° C.

8. The method for preparing a spoke-type non-pneumatic tire according to claim 7, characterized in that: The preparation of the adhesive comprises: Producing the A component; Producing the B component; The component A and the component B are uniformly mixed in a ratio of 100:30-100:80 to obtain the adhesive.

9. The method for preparing a spoke-type non-pneumatic tire according to claim 8, characterized in that: The preparation of the A component comprises: The olefin rubber is kneaded at 50-60° C. for a period of time, then heated to 80-90° C., the antioxidant, the accelerator, the activator and the reinforcing agent are added, and the kneading is continued and the temperature is raised to 150-160° C., and the rubber is discharged to obtain a first rubber compound; The first rubber material is kept at 20-25° C. for a period of time, then heated to 50-60° C., the cross-linking agent is added and the rubber material is kneaded for a period of time, and then heated to 90-100° C. to produce the rubber material, thereby obtaining the second rubber material. The second rubber material and the A solvent are uniformly mixed to obtain the A component.

10. The method for preparing a spoke-type non-pneumatic tire according to claim 8, characterized in that: The preparation of the B component comprises: Dehydrating the epoxy resin at 110-120° C. to obtain a dehydrated epoxy resin; After cooling the dehydrated epoxy resin to 50-60° C., adding the fatty amine to obtain a modified epoxy resin; After cooling the modified epoxy resin to 20-30° C., adding the solvent B and mixing evenly to obtain a uniform solution; Dehydrating the polyol at 110-120° C. to obtain a dehydrated polyol; After cooling the dehydrated polyol to 50-60° C., adding the isocyanate to obtain a mixture containing an isocyanate group at the end and an isocyanate; The mixture containing isocyanate groups at the ends and isocyanate is mixed evenly with the uniform solution, and reacted at 30-40° C. for a period of time to obtain the B component.

Citation Information

Patent Citations

  • Detachable airless tire for improving driver's comfort

    CN107199831A

  • Adhesive composition for tire cord, tire cord, and tire

    CN114651051A

  • Non-pneumatic tire bonding material as well as preparation method and application thereof

    CN114907791A

  • Single-component polyurethane adhesive as well as preparation method and application thereof

    CN115926714A

  • Single-component polyurethane adhesive and preparation method thereof

    CN117210184A