OCA optical cement composition, OCA optical cement film and thin-film solar cell

By using OCA optical glue composition as transparent conductive layer in thin-film solar cells, the problem of aging of traditional thin-film solar cell materials is solved, the photoelectric conversion efficiency and service life are improved, and the conductivity is significantly improved.

CN118995092AInactive Publication Date: 2024-11-22JETAYO TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411107909.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The transparent conductive layer of traditional thin-film solar cells has aging due to ultraviolet rays and environmental factors during long-term outdoor use, affecting the photoelectric conversion efficiency and service life.

Method used

OCA optical glue is prepared by distillation and cross-linking reaction using a composition of OCA optical glue, including acrylate monomers, catalysts, curing agents, tackifying resins, ultraviolet absorbers, quenchers, free radical capture agents and antioxidants. The film enhances its stability and durability and is used as a transparent conductive layer in thin-film solar cells.

Benefits of technology

It improves the photoelectric conversion efficiency and service life of thin-film solar cells, enhances the conductivity, avoids the aging of the conductive layer, improves the photoelectric conversion efficiency by 15%, and maintains a 12% conductive effect after 10 years.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995092A_ABST
    Figure CN118995092A_ABST
Patent Text Reader

Abstract

The invention provides an OCA optical cement composition, an OCA optical cement film and a thin-film solar cell, and relates to the technical field of solar cell application. 5 to 10 parts of a catalyst; 5-10 parts of a curing agent; 5 to 10 parts of tackifying resin; 5-10 parts of an ultraviolet light absorber; 1-5 parts of a quenching agent; 1-5 parts of a free radical trapping agent; 1-3 parts of an antioxidant; in the preparation process of the composition of the OCA, the light-cured resin is added, so that the composition can be rapidly cured under the action of UV light, the production efficiency is improved, the stable adhesive property is formed, the production cycle is shortened, the weather resistance and mechanical strength of a final product can be enhanced, and the application range of the composition of the OCA is widened. The method is suitable for applications requiring rapid production and high durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cell applications, and in particular to an OCA optical adhesive composition, an OCA optical adhesive film and a thin-film solar cell. Background Art

[0002] OCA optical adhesive is a colorless, transparent special adhesive with a light transmittance of more than 90%. It has excellent bonding strength and small curing shrinkage. Its main composition includes acrylic OCA adhesive or silicone OCA adhesive. These materials are coated on optical grade transparent substrates in a dissolved state, and then optical release films are attached to the upper and lower surfaces to form double-sided tapes.

[0003] Thin-film solar cells are a thin and flexible solar power generation technology. Their advantages are that they can be closely integrated with various lightweight roofs and walls, and the photoelectric conversion efficiency is continuously improved. This technology is mainly used in the field of new energy, especially the research and application of solar power generation technology. The main challenge currently faced is that the optical adhesive film used in the transparent conductive layer of traditional thin-film solar cells will age due to ultraviolet rays and other environmental factors under long-term outdoor use conditions, affecting the photoelectric conversion efficiency and service life. Therefore, the present invention proposes a composition of OCA optical adhesive, OCA optical adhesive film and thin-film solar cells. Summary of the invention

[0004] The purpose of the present invention is to solve the shortcomings of the prior art and to provide an OCA optical adhesive composition, an OCA optical adhesive film and a thin-film solar cell.

[0005] In order to achieve the above object, the present invention adopts the following technical solution: The composition of OCA optical adhesive specifically includes the following components:

[0006] Acrylate monomer: 15-30 parts;

[0007] Catalyst: 5-10 parts;

[0008] Curing agent: 5-10 parts;

[0009] Tackifying resin: 5-10 parts;

[0010] Ultraviolet absorber: 5-10 parts;

[0011] Quencher: 1-5 parts;

[0012] Free radical scavenger: 1-5 parts;

[0013] Antioxidants: 1-3 parts;

[0014] Photocurable resin: 2-6 parts. The specific preparation method of the composition of the OCA optical adhesive is as follows:

[0015] S1. Treating monofunctional methyl acrylate by distillation to remove polymerization inhibitor, water and other impurities in the monofunctional methyl acrylate, mixing the treated monofunctional methyl acrylate with 0.1% to 2% of persulfate by weight to carry out polymerization reaction, adding a catalyst in the process, wherein the catalyst is dibutyltin diacetate catalyst, and the ratio is 10:4. After a period of reaction, adding p-hydroxyanisole to stop the polymerization reaction, distilling again to improve the purity and storage stability of the high prepolymer, thereby completing the preparation of the acrylate prepolymer;

[0016] S2. The acrylate prepolymer prepared in step S1 is mixed with the tackifying resin, a curing agent is added, and the mixture is stirred thoroughly to form a uniform base liquid of the OCA optical adhesive.

[0017] S3. After adding the curing agent and stirring for a period of time, add the photocuring resin into the mixed solution and stir for 5 minutes. Then, add the ultraviolet absorber, quencher and free radical scavenger in sequence. The addition interval is 2 minutes. After continuous stirring and mixing, add the antioxidant and stir for 15 minutes. After the raw materials in the solution are completely and evenly mixed, the base glue of the finished COA optical glue is obtained.

[0018] Preferably, in step S2, the base solution of the acrylate prepolymer and the tackifying resin is ethyl acetate, and the ratio of the acrylate prepolymer, tackifying resin, ethyl acetate, curing agent, photocurable resin, ultraviolet absorber, quencher, free radical scavenger and antioxidant is 10:4:5:2:1:2:1.5:1:1.

[0019] OCA optical adhesive film, the preparation method of the OCA optical adhesive film is as follows:

[0020] a. The OCA optical adhesive prepared in step S3 is evenly applied on the PET film;

[0021] b. Send the coated PET film into a drying channel to evaporate the base liquid of the OCA optical adhesive to form a uniform OCA adhesive layer;

[0022] c. By heating, the cross-linking reaction between the acrylate prepolymer and the curing agent is fully carried out to form a stable three-dimensional network structure and achieve complete curing;

[0023] d. The prepared OCA optical adhesive composition is tested for appearance, thickness, transmittance and viscosity, and then rolled up to complete the preparation of the OCA optical adhesive composition.

[0024] Preferably, the PET film described in step a needs to be corona treated in advance to increase its surface energy and ensure that the glue can be evenly distributed. In step b, the temperature range of the PET film in the drying channel is 60°C-120°C, and the temperature at which the cross-linking reaction between the acrylate prepolymer and the curing agent is fully carried out in step c is adjusted to 90°C-120°C.

[0025] Preferably, a detection component is also included, which includes a detection platform, a laser rangefinder, a camera component, a housing, and a pressure sensor and a winding component in the housing;

[0026] The winding assembly is respectively fixed on both sides of the detection table, the camera assembly is fixed on the surface of the detection table, laser rangefinders and shells are respectively arranged on the detection tables on both sides of the camera assembly, a pressure sensor is arranged inside the shell, the OCA optical film is located between the surface of the detection table and the laser rangefinder, the camera assembly and the pressure sensor, and the OCA optical film is fixed on the winding assembly.

[0027] Preferably, the processing steps of the surface image information of the OCA optical film are as follows: the image information of the surface and the back of the OCA optical film is photographed by a camera component, the image is then preprocessed, and then the feature points of the image are extracted, the feature points are the stain features on the surface of the OCA optical film, and the stains have obvious differences in color from the surface of the OCA optical film. Therefore, by extracting the stain features on the surface of the OCA optical film, it is determined whether the transmittance of the OCA optical film meets the standard. When the proportion of the stain features of the OCA optical film to the surface of the OCA optical film exceeds 1%, it indicates that the transmittance of the OCA optical film does not meet the standard.

[0028] Preferably, the specific detection steps of the pressure sensor are as follows: when the OCA optical film passes through the detection surface of the pressure sensor, when there are bubbles on the surface of the OCA optical film, the bulge of the bubbles will cause the detection surface of the pressure sensor to be subjected to pressure, thereby testing whether there are bubbles on the surface of the OCA optical film.

[0029] Preferably, the specific steps for detecting the thickness of the OCA optical adhesive film are as follows: use a laser rangefinder to detect the distance between it and the surface of the OCA optical adhesive film, and then subtract the distance between the laser rangefinder and the surface of the OCA optical adhesive film from the distance between the laser rangefinder and the surface of the detection table to calculate the thickness of the OCA optical adhesive film, thereby completing the thickness detection of the OCA optical adhesive film.

[0030] A thin-film solar cell comprises an OCA optical adhesive composition and an OCA optical adhesive film, wherein the OCA optical adhesive composition is the above-mentioned OCA optical adhesive composition, and the OCA optical adhesive film is the above-mentioned OCA optical adhesive film.

[0031] Compared with the prior art, the advantages and positive effects of the present invention are:

[0032] 1. In the process of preparing the composition of OCA optical adhesive in the present invention, by adding a photocurable resin, it can be quickly cured under the action of UV light, improve production efficiency, and form stable bonding performance. The addition of this material not only shortens the production cycle, but also enhances the weather resistance and mechanical strength of the final product, and is suitable for applications requiring rapid production and high durability. Secondly, in the process of preparing the composition of CA optical adhesive in the present invention, ultraviolet absorbers, quenchers, free radical scavengers and antioxidants are added. The antioxidant can further improve the processing performance and durability of the OCA optical adhesive. The ultraviolet absorber can absorb harmful ultraviolet light, improve the efficiency of solar energy conversion to electrical energy, and convert it into heat release. The quencher slows down the photooxidation process by quenching singlet oxygen and free radical capture. The free radical scavenger captures the free radicals generated during the photodegradation process to block the chain reaction. This design makes the OCA optical adhesive prepared by the present invention Compared with traditional optical adhesive compositions, the composition of A optical adhesive has high stability, high oxidation resistance, longer service life and is not easily affected by its own properties over time. The optical adhesive film in the present invention serves as a transparent conductive layer of a thin-film solar cell, and has high stability, high lifespan and better light-guiding effect, so that after the optical adhesive film in the present invention is applied to the transparent conductive layer of a thin-film solar cell, the light absorption conversion efficiency of the thin-film solar cell is better, and the efficiency of photoelectric conversion is effectively improved. At the same time, the extremely high stability and oxidation resistance can avoid the aging of the conductive layer due to long-term outdoor use, thereby affecting the photoelectric conversion efficiency. Compared with the conductive efficiency of traditional thin-film solar cells, after the optical adhesive film in the present invention is applied to a thin-film solar cell, its conductivity can be improved by 15% compared with traditional thin-film solar cells. This improvement effect still has a 12% improvement in conductivity after 10 years of use.

[0033] 2. In the present invention, when testing the OCA optical film, a laser rangefinder is used to detect the thickness of the OCA optical film, and a camera component is used to capture basic information of the OCA optical film. Image processing is then used to determine the presence of stains on the surface of the OCA optical film, thereby further determining its light transmittance. A pressure sensor can accurately detect whether there are bubbles on the surface of the OCA optical film. The above design is used to detect the quality of the OCA optical film, and precise data is used to achieve a detailed detection of the quality of the OCA optical film. Compared with traditional detection by the naked eye, the detection data in the present invention is more standardized and more targeted. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Schematic diagram of the detection process of the OCA optical adhesive film of the present invention.

[0035] Legend:

[0036] 1. Testing table; 2. Laser rangefinder; 3. Camera assembly; 4. Pressure sensor; 5. Shell; 6. Winding assembly. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] The present invention provides a technical solution: a composition of OCA optical adhesive, specifically comprising the following components:

[0040] Acrylate monomer: 20 parts;

[0041] Catalyst: 8 parts;

[0042] Curing agent: 4 parts;

[0043] Tackifying resin: 8 parts;

[0044] UV absorber: 2 parts;

[0045] Quencher: 3 parts;

[0046] Free radical scavenger: 2 parts;

[0047] Antioxidants: 2 parts;

[0048] Photocurable resin: 2 parts. The specific preparation method of the composition of the OCA optical adhesive is as follows:

[0049] S1. Treating monofunctional methyl acrylate by distillation to remove polymerization inhibitor, water and other impurities in the monofunctional methyl acrylate, mixing the treated monofunctional methyl acrylate with 0.4 parts by weight of initiator persulfate to carry out polymerization reaction, adding a catalyst in the process, wherein the catalyst is dibutyltin diacetate catalyst, and the ratio is 10:4. After a period of reaction, adding p-hydroxyanisole to stop the polymerization reaction, distilling again to improve the purity and storage stability of the high prepolymer, thereby completing the preparation of the acrylate prepolymer;

[0050] S2. The acrylate prepolymer prepared in step S1 is mixed with a tackifying resin, and a curing agent is added to promote the cross-linking and curing of the prepolymer to form a stable adhesive layer. The mixture is fully stirred to form a uniform base liquid of the OCA optical adhesive.

[0051] Step S3, after adding the curing agent and stirring for a period of time, add the photocurable resin into the mixed solution, stir for 5 minutes, then add the ultraviolet absorber, quencher and free radical scavenger in sequence, with an addition interval of 2 minutes. After continuous stirring and mixing, add the antioxidant and stir for 15 minutes. After the raw materials in the solution are completely and evenly mixed, the base glue of the finished COA optical glue is obtained.

[0052] Among them, in step S2, the basic solution of the mixture of acrylate prepolymer and tackifying resin is ethyl acetate, and the ratio of acrylate prepolymer, tackifying resin, ethyl acetate, curing agent, photocuring resin, ultraviolet absorber, quencher, free radical scavenger and antioxidant is: 10:4:5:2:1:2:1.5:1:1.

[0053] In this embodiment, by adding a photocurable resin, it can be quickly cured under the action of UV light, improve production efficiency, and form stable bonding performance. The addition of this material not only shortens the production cycle, but also enhances the weather resistance and mechanical strength of the final product, and is suitable for applications that require rapid production and high durability. Secondly, in the present invention, ultraviolet absorbers, quenchers, free radical scavengers and antioxidants are added during the preparation of the composition of CA optical adhesive. The antioxidant can further improve the processing performance and durability of OCA optical adhesive. The ultraviolet absorber can absorb harmful ultraviolet light and convert it into heat release. The quencher slows down the photooxidation process by quenching singlet oxygen and free radical capture. The free radical scavenger captures the free radicals generated during the photodegradation process and blocks the chain reaction; Singlet oxygen quenching: Singlet oxygen is a highly active oxygen species that can react with many substances, resulting in oxidative degradation of the material. The quencher can react with singlet oxygen and convert it into more stable triplet oxygen or other inactive forms, thereby protecting the material from oxidative damage. Free radical capture: During the photodegradation process, the material may produce free radicals, which can trigger chain reactions and cause the material performance to deteriorate. Free radical scavengers can react with free radicals to form stable compounds, thereby blocking the chain reaction and slowing down the degradation rate of the material. Improved stability: By adding quenchers and free radical scavengers, the composition of OCA optical adhesive can resist the negative effects of external environmental factors (such as light, temperature, humidity, etc.) and maintain the stability of its physical and chemical properties. Antioxidant property: The addition of quenchers and free radical scavengers significantly improves the antioxidant properties of OCA optical adhesive and reduces problems such as yellowing and hardening caused by oxidation. Extended service life: Due to the protective effect of quenchers and free radical scavengers, the service life of OCA optical adhesive is extended, and good bonding and optical properties can be maintained even after long-term use. Keeping properties unchanged over time: Traditional optical adhesives may degrade over time, but OCA optical adhesives containing quenchers can better maintain their properties, including transparency, refractive index and bonding strength. Wide application: OCA optical adhesive with high stability and oxidation resistance can be widely used in various optical products, such as touch screens, displays, optical lenses, etc., to improve the reliability and durability of the products. This design makes the OCA optical adhesive composition prepared by the present invention have high stability and oxidation resistance compared with traditional optical adhesive compositions, and has a longer service life and is not easily affected by its own properties over time.

[0054] Example 2

[0055] like Figure 1 As shown, the OCA optical adhesive film, the preparation method of the OCA optical adhesive film is as follows:

[0056] a. The OCA optical adhesive prepared in step S2 is evenly applied on the PET film;

[0057] b. Send the coated PET film into a drying channel to evaporate the base liquid of the OCA optical adhesive to form a uniform OCA adhesive layer;

[0058] c. By heating, the cross-linking reaction between the acrylate prepolymer and the curing agent is fully carried out to form a stable three-dimensional network structure and achieve complete curing;

[0059] d. The prepared OCA optical adhesive composition is tested for appearance, thickness, transmittance and viscosity, and then rolled up to complete the preparation of the OCA optical adhesive composition.

[0060] The PET film described in step a needs to be corona treated in advance to increase its surface energy and ensure that the glue can be evenly distributed. In step b, the temperature range of the PET film in the drying channel is 60°C-120°C. In step c, the temperature at which the cross-linking reaction between the acrylate prepolymer and the curing agent is fully carried out is adjusted to 90°C-120°C.

[0061] The detection assembly includes a detection platform 1, a laser rangefinder 2, a camera assembly 3, a housing 5, a pressure sensor 4 in the housing 5, and a winding assembly 6;

[0062] The winding assembly 6 is respectively fixed on both sides of the detection platform 1, the camera assembly 3 is fixed on the surface of the detection platform 1, and the detection platforms on both sides of the camera assembly 3 are respectively provided with a laser rangefinder 2 and a housing 5, and a pressure sensor 4 is arranged inside the housing 5. The OCA optical adhesive film is located between the surface of the detection platform 1 and the laser rangefinder 2, the camera assembly 3 and the pressure sensor 4, and the OCA optical adhesive film is fixed on the winding assembly 6;

[0063] The specific detection principle of the detection component is as follows: first, the OCA optical film is placed on the surface of the detection platform 1, located between the camera component 3, the laser rangefinder 2 pressure sensor and the detection platform 1, the bottom of the OCA optical film is attached to the surface of the detection platform 1, and one end of the OCA optical film is fixed on the winding component 6, and the winding component 6 is symmetrically arranged on both sides of the detection platform 1. The winding component 6 consists of a winding motor and a winding roller, and then the OCA optical film is sequentially driven on the surface of the detection platform 1. When the OCA optical film passes through the surface of the detection platform 1, the laser rangefinder 2 is used to measure the distance between it and the surface of the OCA optical film, the camera component 3 is used to capture the image information of the surface of the OCA optical film, and the pressure sensor 4 is used to detect whether there are bubbles on the surface of the OCA optical film. Then, the OCA optical film is turned over and fixed on the winding component 6 on the other side of the detection platform 1, and is driven in the opposite direction, that is, the back of the OCA optical film is detected. The specific steps can be repeated as above;

[0064] The instrument is beneficial for collecting basic information of the OCA optical adhesive film, and then performing data processing based on the collected basic information of the OCA optical adhesive film, and judging whether the OCA optical adhesive film meets the standards according to the result of the data processing, and then judging whether it can be used in thin-film solar cells.

[0065] Among them, the processing steps of the surface image information of the OCA optical film are as follows: the camera component 3 captures the image information of the surface and the back of the OCA optical film, and then pre-processes the image, and then extracts the feature points of the image. The feature points are the stain features on the surface of the OCA optical film. The stains have obvious differences in color from the surface of the OCA optical film. Therefore, by extracting the stain features on the surface of the OCA optical film, it is determined whether the transmittance of the OCA optical film meets the standard. When the stain features of the OCA optical film account for more than 1% of the surface of the OCA optical film, it indicates that the transmittance of the OCA optical film does not meet the standard.

[0066] Among them, the specific detection steps of the pressure sensor 4 are as follows: when the OCA optical film passes through the detection surface of the pressure sensor 4, when there are bubbles on the surface of the OCA optical film, the bubbles bulge, causing the detection surface of the pressure sensor 4 to be subjected to pressure, thereby testing whether there are bubbles on the surface of the OCA optical film.

[0067] Among them, the specific steps for detecting the thickness of the OCA optical film are as follows: use the laser rangefinder 2 to detect the distance between it and the surface of the OCA optical film, and then subtract the distance between the laser rangefinder 2 and the surface of the OCA optical film from the distance between the laser rangefinder 2 and the surface of the detection platform 1 to calculate the thickness of the OCA optical film, and complete the thickness detection of the OCA optical film. When performing the detection, not only the distance between the surface of the OCA optical film and the laser rangefinder 2 is detected, but also when detecting the data information on the back of the OCA optical film, the distance between the laser rangefinder 2 and the back of the OCA optical film is further measured, and the data of the two measurements are used for calibration to further improve the accuracy of the data.

[0068] In this embodiment, a laser rangefinder 2 is used to detect the thickness of the OCA optical film, and a camera assembly 3 is used to capture basic information of the OCA optical film. Image processing is then used to determine the presence of stains on the surface of the OCA optical film, thereby further determining its light transmittance. A pressure sensor 4 is able to accurately detect whether there are bubbles on the surface of the OCA optical film. The above design is used to detect the quality of the OCA optical film, and precise data is used to achieve a detailed detection of the quality of the OCA optical film. Compared with traditional detection by the naked eye, the detection data in the present invention is more standardized and more targeted.

[0069] Example 3

[0070] A thin-film solar cell comprises an OCA optical adhesive composition and an OCA optical adhesive film, wherein the OCA optical adhesive composition is the OCA optical adhesive composition described above, and the OCA optical adhesive film is the OCA optical adhesive film described above.

[0071] The above description is only a preferred embodiment of the present invention and does not limit the present invention in other forms. Any technician familiar with the profession may use the technical content disclosed above to change or modify it into an equivalent embodiment with equivalent changes and apply it to other fields. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. Composition of OCA optical adhesive, It is characterized in that Specifically include the following weight parts: Acrylate monomer: 15-30 parts; Catalyst: 5-10 parts; Curing agent: 5-10 parts; Tackifying resin: 5-10 parts; Ultraviolet absorber: 5-10 parts; Quencher: 1-5 parts; Free radical scavenger: 1-5 parts; Antioxidants: 1-3 parts; Photocurable resin: 2-6 parts. The specific preparation method of the composition of the OCA optical adhesive is as follows: S1. Treating monofunctional methyl acrylate by distillation to remove polymerization inhibitor, water and other impurities in the monofunctional methyl acrylate, mixing the treated monofunctional methyl acrylate with 0.1% to 2% of persulfate by weight to carry out polymerization reaction, adding a catalyst in the process, wherein the catalyst is dibutyltin diacetate catalyst, and the ratio is 10:

4. After a period of reaction, adding p-hydroxyanisole to stop the polymerization reaction, distilling again to improve the purity and storage stability of the high prepolymer, thereby completing the preparation of the acrylate prepolymer; S2, the acrylate prepolymer prepared in step S1 is mixed with the tackifying resin, a curing agent is added, and the mixture is stirred thoroughly to form a uniform base liquid of the OCA optical adhesive; S3. After adding the curing agent and stirring for a period of time, add the photocuring resin into the mixed solution and stir for 5 minutes. Then, add the ultraviolet absorber, quencher and free radical scavenger in sequence. The addition interval is 2 minutes. After continuous stirring and mixing, add the antioxidant and stir for 15 minutes. After the raw materials in the solution are completely and evenly mixed, the base glue of the finished COA optical glue is obtained.

2. The composition of OCA optical adhesive according to claim 1, Features: In step S2, the base solution of the acrylate prepolymer and the tackifying resin is ethyl acetate, and the weight ratio of the acrylate prepolymer, tackifying resin, ethyl acetate, curing agent, photocuring resin, ultraviolet absorber, quencher, free radical scavenger and antioxidant is 10:4:5:2:1:2:1.5:1:

1.

3. An OCA optical adhesive film, prepared using the OCA optical adhesive composition according to any one of claims 1 to 2, Features: The preparation method of the OCA optical adhesive film is specifically as follows: a. The OCA optical adhesive prepared in step S3 is evenly applied on the PET film; b. Send the coated PET film into a drying channel to evaporate the base liquid of the OCA optical adhesive to form a uniform OCA adhesive layer; c. By heating, the cross-linking reaction between the acrylate prepolymer and the curing agent is fully carried out to form a stable three-dimensional network structure and achieve complete curing; d. The prepared OCA optical adhesive composition is tested for appearance, thickness, transmittance and viscosity, and then rolled up to complete the preparation of the OCA optical adhesive composition.

4. The OCA optical adhesive film according to claim 3, Features: The PET film described in step a needs to be corona treated in advance to increase its surface energy and ensure that the glue can be evenly distributed. In step b, the temperature range of the PET film in the drying channel is 60°C-120°C. In step c, the temperature at which the cross-linking reaction between the acrylate prepolymer and the curing agent is fully carried out is adjusted to 90°C-120°C.

5. The OCA optical adhesive film detection component according to claim 4, Features: It comprises a detection platform (1), a laser rangefinder (2), a camera assembly (3), a housing (5), and a pressure sensor (4) and a winding assembly (6) inside the housing (5); The winding assembly (6) is respectively fixed on both sides of the detection platform (1); the camera assembly (3) is fixed on the surface of the detection platform (1); laser rangefinders (2) and shells (5) are respectively arranged on the detection platforms on both sides of the camera assembly (3); a pressure sensor (4) is arranged inside the shell (5); an OCA optical adhesive film is located between the surface of the detection platform (1) and the laser rangefinder (2), the camera assembly (3) and the pressure sensor (4); and the OCA optical adhesive film is fixed on the winding assembly (6).

6. The specific steps of processing the image information of the surface of the OCA optical adhesive film using the detection component of the OCA optical adhesive film described in claim 5 are as follows: the image information of the surface and the back of the OCA optical adhesive film is photographed by the camera component (3), and then the image is preprocessed, and then the feature points of the image are extracted. The feature points are the stain features on the surface of the OCA optical adhesive film. The color of the stain is significantly different from that of the surface of the OCA optical adhesive film. Therefore, by extracting the stain features on the surface of the OCA optical adhesive film, it is determined whether the transmittance of the OCA optical adhesive film meets the standard. When the proportion of the stain features of the OCA optical adhesive film to the surface of the OCA optical adhesive film exceeds 1%, it indicates that the transmittance of the OCA optical adhesive film does not meet the standard.

7. The steps of using the OCA optical adhesive film detection component described in claim 5 to detect whether there are bubbles on the surface of the OCA optical adhesive film are as follows: when the OCA optical adhesive film passes through the detection surface of the pressure sensor (4), when there are bubbles on the surface of the OCA optical adhesive film, the bubbles bulge, causing the detection surface of the pressure sensor (4) to be subjected to pressure, thereby testing whether there are bubbles on the surface of the OCA optical adhesive film.

8. The specific steps of using the OCA optical adhesive film detection component of claim 5 to detect the thickness of the OCA optical adhesive film are as follows: using a laser rangefinder (2) to detect the distance between it and the surface of the OCA optical adhesive film, and then subtracting the distance between the laser rangefinder (2) and the surface of the detection platform (1) from the distance between the laser rangefinder (2) and the surface of the OCA optical adhesive film to calculate the thickness of the OCA optical adhesive film, thereby completing the thickness detection of the OCA optical adhesive film.

9. Thin film solar cells, Features: The OCA optical adhesive film comprises the OCA optical adhesive film as described in any one of claims 3 to 4, and the OCA optical adhesive film is applied to the transparent conductive layer of a thin-film solar cell.

Citation Information

Patent Citations

  • Acrylate OCA optical adhesive film, and preparation method and application thereof

    CN106590484A

  • Intelligent visual detection mechanism of optical film

    CN107449785A

  • Anti-yellowing OCA optical adhesive

    CN110894402A

  • Optical adhesive as well as preparation method and application thereof

    CN117285877A

  • Optical clear adhesive and manufacturing method thereof

    US20200239744A1