Hot-melt pressure-sensitive adhesive for automotive interior sponge cushion and preparation method of hot-melt pressure-sensitive adhesive

By using a specific combination of hot melt pressure-sensitive adhesive preparation method on the sponge cushion of the car interior, the problem of adhesive lifting and bounceing on uneven surfaces is solved, providing an efficient and environmentally friendly bonding solution, suitable for a variety of Soft structure splicing and reduce environmental impacts in production and use.

CN118995098APending Publication Date: 2024-11-22RUGAO JIAHAO HOT MELT ADHESIVE

Patent Information

Application Number
CN202411373122.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The adhesive glue of existing automotive interior sponge cushions is prone to rise and pop when dealing with uneven substrate surfaces, and lacks environmentally friendly alternatives, making it difficult to meet the demand for environmentally friendly glue in the new energy vehicle industry.

Method used

The preparation method of hot melt pressure-sensitive adhesive using parts by weight includes main polymers (styrene block copolymers and butyl rubber), tackifying resins (hydrogenated C5/C9 copolymer resins and hydrogenated rosin resins) and antioxidants. Adhesives with high wetting properties and small angle peel strength are prepared by specific mass ratios and process steps (premelting, heating, stirring, vacuuming).

Benefits of technology

It improves the bonding strength, wetting and high temperature resistance of hot melt pressure-sensitive adhesive, reduces odor and VOC content, and is suitable for soft structure splicing of automobiles, sofas and office seats, and has no waste emissions, which meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives, in particular to a hot-melt pressure-sensitive adhesive for an automotive interior sponge cushion, which is prepared from the following raw materials in parts by weight: 27 to 35 parts of main polymer, 37 to 50 parts of tackifying resin, 15 to 25 parts of petroleum rubber oil and 0.2 to 0.5 part of antioxidant, the main polymer comprises a styrene block copolymer and butyl rubber. The specific hydrogenated resin, monomer resin and butyl rubber are introduced, so that the hot-melt pressure-sensitive adhesive has sufficient wettability when used for treating some uneven substrate surfaces, is excellent in leveling property during coating, and can be applied to splicing and bonding of soft structures of automobile seats, soft structures of sofas, soft structures of office seats and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesives, and in particular to a hot-melt pressure-sensitive adhesive for automobile interior sponge cushions and a preparation method thereof. Background Art

[0002] With the advancement of modernization, civilian cars have become a necessary means of transportation for people's daily lives. At present, the adhesives that can be used for automobile-related accessories include water-based acrylic adhesive, oil-based acrylic adhesive, oil-based polyurethane, EVA, etc.

[0003] With the rapid development of the new energy vehicle industry in China and the increasing environmental pressure in recent years, the automotive-related industries have an increasingly strong demand for environmentally friendly glue.

[0004] At present, there is usually a layer of foam soft structure inside the car seat, and this structure is wrapped with a layer of leather or fabric surface. But before wrapping the surface layer, this soft structure is made by bonding the punched backrest part and the seat cushion part with adhesives. The current mature product is oil-based polyurethane adhesive.

[0005] For environmental considerations, an environmentally friendly hot-melt pressure-sensitive adhesive needs to be developed to replace oil-based adhesives for the internal foam structure of car seats. Since the surface energy of the foam material is low and the seat has a curved structure, the hot-melt pressure-sensitive adhesive needs to have sufficient wettability and small-angle peel strength, light color, and low odor.

[0006] Chinese invention patent CN107099265B discloses a hot melt adhesive for automotive interior parts and its preparation method, which can be used for bonding different materials, especially suitable for bonding the interlayer metal plate of refrigerated trucks to PU foam materials. However, when processing some uneven substrate surfaces, the adhesive is prone to warping and bouncing. Summary of the invention

[0007] In order to solve the problems in the prior art, the first aspect of the present invention provides a hot melt pressure-sensitive adhesive for automotive interior sponge seat cushions, the preparation raw materials of which include, by weight: 27-35 parts of a main polymer, 37-50 parts of a tackifying resin, 15-25 parts of a petroleum-based rubber oil, and 0.2-0.5 parts of an antioxidant; the main polymer includes a styrene block copolymer and butyl rubber.

[0008] In one embodiment, the host polymer is a styrene block copolymer and butyl rubber.

[0009] In one embodiment, the styrene block copolymer includes any one of styrene-isoprene-styrene block copolymer (SIS), styrene-butadiene-styrene block copolymer (SBS), and styrene-ethylene-butylene-styrene block copolymer (SEBS).

[0010] In one embodiment, the styrenic block copolymer is SIS.

[0011] In one embodiment, the structure of the SIS includes any one of a linear structure and a star structure, and the diblock content of the SIS is 20-50%.

[0012] In one embodiment, the SIS is a linear structure, the diblock content of the SIS is 50%, and it is purchased from Baling Petrochemical with a grade of YH-1126.

[0013] In one embodiment, the butyl rubber includes one or more of BK-1765N, BK-1675N, and BK-1675T.

[0014] In one embodiment, the butyl rubber is BK-1765N.

[0015] In one embodiment, the BK-1765N is purchased from Kasvik, Russia.

[0016] In one embodiment, the mass ratio of the styrene block copolymer to the butyl rubber is (25-30):(2-5).

[0017] In one embodiment, the mass ratio of the styrene block copolymer to the butyl rubber is 14:1.

[0018] In one embodiment, the tackifying resin includes one or both of a hydrogenated resin and a monomeric resin.

[0019] In one embodiment, the tackifying resin is a hydrogenated resin and a monomeric resin.

[0020] In one embodiment, the hydrogenated resin includes hydrogenated products of any two of C5 petroleum resin, C9 petroleum resin, C5 / C9 copolymer resin, and rosin resin.

[0021] In one embodiment, the hydrogenated resin is a hydrogenated C5 / C9 copolymer resin and a hydrogenated rosin resin; the mass ratio of the hydrogenated C5 / C9 copolymer resin to the hydrogenated rosin resin is (6-7):(1-2).

[0022] In one embodiment, the mass ratio of the hydrogenated C5 / C9 copolymer resin to the hydrogenated rosin resin is 35:9.

[0023] In one embodiment, the mass ratio of the monomer resin to SIS is (2-5): (25-30).

[0024] In one embodiment, the mass ratio of the hydrogenated C5 / C9 copolymer resin, the monomer resin, and the hydrogenated rosin resin is (30-35):(2-5):(5-10).

[0025] In one embodiment, the mass ratio of the hydrogenated C5 / C9 copolymer resin, the monomer resin, and the hydrogenated rosin resin is 35:5:9.

[0026] In one embodiment, the hydrogenated C5 / C9 copolymer resin includes HM-1000, which is available from Henghe Technology Materials Co., Ltd.

[0027] In one embodiment, the monomer resin is Kristalex5140, purchased from Eastman, USA.

[0028] In one embodiment, the softening point of the hydrogenated rosin resin is 98-110°C.

[0029] In one embodiment, the softening point of the hydrogenated rosin resin is 98-108° C. The hydrogenated rosin resin is KA100W, purchased from Guangdong Kemao Forestry Chemical Co., Ltd.

[0030] In one embodiment, the cyclopentane rubber oil includes one or more of cyclopentane oil N4006, cyclopentane oil N4010, and cyclopentane oil N4016.

[0031] In one embodiment, the cycloalkane rubber oil is cycloalkane oil N4010 purchased from PetroChina.

[0032] In one embodiment, the antioxidant includes at least one of a hindered phenol antioxidant and a phosphite antioxidant.

[0033] In one embodiment, the antioxidant comprises a hindered phenolic antioxidant.

[0034] In one embodiment, the hindered phenol antioxidant is one or more of 1076, 1010, 1790, and 1098.

[0035] The second aspect of the present invention provides a method for preparing a hot melt pressure-sensitive adhesive for automobile interior sponge seat cushions, comprising the following steps: stirring and heating a main polymer, petroleum rubber oil, an antioxidant and a tackifying resin to obtain a hot melt pressure-sensitive adhesive for automobile interior sponge seat cushions.

[0036] In one embodiment, the preparation method comprises the following specific steps:

[0037] S1: pre-melting butyl rubber at 150°C through a mixing device;

[0038] S2: Heat the petroleum rubber oil bath to 110-115°C for 5-10 minutes, and control the stirring speed at 20-30r / min;

[0039] S3: Add SIS and antioxidant and heat electrically to 120-125°C, stir for 9-11 minutes, then vacuum and heat to 130-135°C, stir for 30-40 minutes until the rubber particles are completely melted; turn off the vacuum, add pre-melted butyl rubber, vacuum and stir for 7-9 minutes;

[0040] S4: Turn off the vacuum, add the monomer resin and stir for 5-10 minutes;

[0041] S5: Add hydrogenated C5 / C9 copolymer resin and hydrogenated rosin resin, evacuate and heat to 145-150°C, turn off the electric heating, increase the stirring speed to 40-50r / min, stir for 30-40 minutes and then turn off the vacuum to obtain.

[0042] In one embodiment, the vacuum degree in S3 and S5 is -0.1 MPa.

[0043] Beneficial Effects

[0044] 1. Based on the system of the present invention, by co-introducing hydrogenated C5 / C9 copolymer resin, hydrogenated rosin resin and monomer resin, especially controlling the mass ratio of the three to be (30-35): (2-5): (5-10), it has good compatibility with other substances in the system, can balance the viscosity of the system, improve the cohesion of the system, and improve the bonding strength of the hot melt pressure-sensitive adhesive finally prepared.

[0045] 2. Based on the system of the present invention, the main polymer is a combination of SIS and butyl rubber, especially the mass ratio of SIS to butyl rubber is (25-30): (2-5), which can make the hot melt pressure-sensitive adhesive have sufficient wettability when treating some uneven substrate surfaces and good leveling properties during coating.

[0046] 3. The preparation method of the hot-melt pressure-sensitive adhesive for high-end Velcro provided by the present invention has no discharge of three wastes during production and use, does not contain organic solvents, and is beneficial to environmental protection.

[0047] 4. In the present invention, by controlling 27-25 parts of a specific main polymer, 37-50 parts of a specific tackifying resin, 15-25 parts of a specific petroleum-based rubber oil, and 0.2-0.5 parts of a specific antioxidant, the wettability, high temperature resistance, and peel strength of the hot melt pressure-sensitive adhesive are improved, and at the same time, the odor of the hot melt adhesive is reduced and the VOC content of the hot melt pressure-sensitive adhesive is reduced.

[0048] 5. The hot-melt pressure-sensitive adhesive prepared by the present invention can be used for splicing and bonding of soft structures of automobile seats, soft structures of sofas, soft structures of office chairs, etc. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The experimental methods in the examples without specifying specific conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.

[0050] Example 1

[0051] The first aspect of this embodiment provides a hot melt pressure-sensitive adhesive for automotive interior sponge seat cushions, the raw materials for its preparation include, by weight: 30 parts of a main polymer, 49 parts of a tackifying resin, 20.7 parts of a petroleum-based rubber oil, and 0.3 parts of an antioxidant; the main polymer is a styrene block copolymer and butyl rubber.

[0052] The main polymers are SIS and butyl rubber.

[0053] The mass ratio of SIS to butyl rubber in the main polymer is 14:1.

[0054] The SIS is a linear structure, has a diblock content of 50%, and is purchased from Baling Petrochemical with a brand name of YH-1126.

[0055] The butyl rubber brand is BK-1765N, purchased from Kasvik, Russia.

[0056] The tackifying resin is a hydrogenated resin and a monomeric resin.

[0057] The hydrogenated resin is hydrogenated C5 / C9 copolymer resin and hydrogenated rosin resin; the mass ratio of the hydrogenated C5 / C9 copolymer resin to the hydrogenated rosin resin is 35:9.

[0058] The mass ratio of the hydrogenated C5 / C9 copolymer resin, the monomer resin and the hydrogenated rosin resin is 35:5:9.

[0059] The hydrogenated C5 / C9 copolymer resin is of the brand HM-1000, purchased from Henghe Technology Materials Co., Ltd.

[0060] The monomer resin is Kristalex5140, purchased from Eastman, USA.

[0061] The hydrogenated rosin resin was purchased from Guangdong Kemao Forestry and Chemical Industry Co., Ltd. with a brand name of KA100W.

[0062] The naphthenic rubber oil is naphthenic oil N4010 purchased from PetroChina.

[0063] The antioxidant is antioxidant 1076, purchased from Shanghai Haipu Chemical.

[0064] A second aspect of the present embodiment provides a method for preparing a hot melt pressure-sensitive adhesive for a car interior sponge seat cushion, comprising the following steps:

[0065] S1: pre-melting butyl rubber at 150°C through a mixing device;

[0066] S2: Heat the petroleum rubber oil bath to 110°C and maintain for 8 min, with the stirring speed controlled at 25 r / min;

[0067] S3: Add SIS and antioxidant and heat to 125℃, stir for 10min, then evacuate to -0.1MPa, heat to 135℃, stir for 35min until the rubber particles are completely melted; turn off the vacuum, add pre-melted butyl rubber, evacuate to -0.1MPa and stir for 8min;

[0068] S4: turn off the vacuum, add the monomer resin and stir for 10 minutes;

[0069] S5: Add hydrogenated C5 / C9 copolymer resin and hydrogenated rosin resin, evacuate and heat to 145°C, the vacuum degree is -0.1MPa, turn off the electric heating, increase the stirring speed to 45r / min, stir for 35min and then turn off the vacuum.

[0070] Example 2

[0071] The specific implementation of this embodiment is the same as that of embodiment 1, except that the raw materials for preparation thereof include, by weight: 30 parts of main polymer, 49 parts of tackifying resin, 20.7 parts of petroleum rubber oil, and 0.3 parts of antioxidant. The main polymer is a styrene block copolymer.

[0072] The styrene block copolymer is SIS.

[0073] The SIS is a linear structure, the diblock content of the SIS is 50%, and it is purchased from Baling Petrochemical with a brand name of YH-1126.

[0074] The tackifying resin is a hydrogenated resin.

[0075] The hydrogenated resin is hydrogenated C5 / C9 copolymer resin and hydrogenated rosin resin; the mass ratio of the hydrogenated C5 / C9 copolymer resin to the hydrogenated rosin resin is 40:9.

[0076] The hydrogenated C5 / C9 copolymer resin is of the brand HM-1000, purchased from Henghe Technology Materials Co., Ltd.

[0077] The hydrogenated rosin resin was purchased from Guangdong Kemao Forestry and Chemical Industry Co., Ltd. with a brand name of KA100W.

[0078] Example 3

[0079] The specific implementation of this embodiment is the same as that of embodiment 1, except that the raw materials for preparation thereof include, by weight: 20 parts of main polymer, 60 parts of tackifying resin, 19.7 parts of petroleum rubber oil, and 0.3 parts of antioxidant. The main polymer is a styrene block copolymer.

[0080] The styrene block copolymer is SIS.

[0081] The SIS is a linear structure, the diblock content of the SIS is 50%, and it is purchased from Baling Petrochemical with a brand name of YH-1126.

[0082] The tackifying resin is a hydrogenated resin and a monomeric resin.

[0083] The hydrogenated resin is hydrogenated C5 / C9 copolymer resin and hydrogenated rosin resin; the mass ratio of the hydrogenated C5 / C9 copolymer resin to the hydrogenated rosin resin is 45:10.

[0084] The mass ratio of the hydrogenated C5 / C9 copolymer resin, the monomer resin and the hydrogenated rosin resin is 45:5:10.

[0085] The hydrogenated C5 / C9 copolymer resin is of the brand HM-1000, purchased from Henghe Technology Materials Co., Ltd.

[0086] The hydrogenated rosin resin was purchased from Guangdong Kemao Forestry and Chemical Industry Co., Ltd. with a brand name of KA100W.

[0087] The monomer resin is Kristalex5140, purchased from Eastman, USA.

[0088] Performance Testing

[0089] Test object: hot melt pressure-sensitive adhesive samples for automobile interior sponge seat cushions prepared in Examples 1-3.

[0090] 1. Ring initial adhesion: Test according to GB / T 31125-2014 adhesive tape initial adhesion test method.

[0091] 2. Peel strength: 90° peel strength is tested according to the test method of peel strength of adhesive tape in GB / T 2792-2014.

[0092] 3. Stickiness: The stickiness time is tested according to the test method of GB / T 4851-2014 for stickiness of adhesive tapes.

[0093] 4. Firmness test: The hot melt pressure-sensitive adhesive samples prepared in Examples 1-3 were placed in a 40°C oven with a 90° corner fitted, and the time it took to bounce back was observed.

[0094] The test data are listed in Table 1.

[0095] Table 1

[0096] Example 1 Example 3 Example 3 <![CDATA[Ring tack force (N / in 2 )]]> 35 32 28 90° peel strength (N / in) 30 13 15 <![CDATA[Holding time (1in 2 , 2kg)]]> >72h 40h >72h Firmness No warping or popping after 48 hours 20h to lift and pop open 18h lift and pop

Claims

1. A hot melt pressure-sensitive adhesive for automotive interior sponge seat cushions, characterized in that: The raw materials for its preparation include, by weight: 27-35 parts of main polymer, 37-50 parts of tackifying resin, 15-25 parts of petroleum rubber oil, and 0.2-0.5 parts of antioxidant; the main polymer includes styrene block copolymer and butyl rubber.

2. The hot melt pressure-sensitive adhesive for automobile interior sponge seat cushion according to claim 1, characterized in that: The main polymer is styrene block copolymer and butyl rubber.

3. The hot melt pressure-sensitive adhesive for automobile interior sponge seat cushion according to claim 2, characterized in that: The styrene block copolymer includes any one of SIS, SBS and SEBS.

4. The hot melt pressure sensitive adhesive for automobile interior sponge seat cushion according to claim 2, characterized in that: The mass ratio of the styrene block copolymer to the butyl rubber is (25-30):(2-5).

5. The hot melt pressure sensitive adhesive for automobile interior sponge seat cushion according to claim 1, characterized in that: The tackifying resin includes one or both of a hydrogenated resin and a monomeric resin.

6. The hot melt pressure sensitive adhesive for automobile interior sponge seat cushion according to claim 5, characterized in that: The hydrogenated resin includes hydrogenated products of any two of C5 petroleum resin, C9 petroleum resin, C5 / C9 copolymer resin and rosin resin.

7. The hot melt pressure sensitive adhesive for automobile interior sponge cushion according to claim 6, characterized in that: The hydrogenated resin is hydrogenated C5 / C9 copolymer resin and hydrogenated rosin resin; the mass ratio of the hydrogenated C5 / C9 copolymer resin to the hydrogenated rosin resin is (6-7):(1-2).

8. The hot melt pressure sensitive adhesive for automobile interior sponge seat cushion according to claim 7, characterized in that: The mass ratio of the hydrogenated C5 / C9 copolymer resin, the monomer resin and the hydrogenated rosin resin is (30-35):(2-5):(5-10).

9. The hot melt pressure sensitive adhesive for automobile interior sponge seat cushion according to claim 1, characterized in that: The petroleum-based rubber oil is cycloalkane rubber oil.

10. A method for preparing a hot melt pressure sensitive adhesive for automobile interior sponge seat cushion according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: stirring and heating a main polymer, petroleum rubber oil, an antioxidant and a tackifying resin to obtain a hot-melt pressure-sensitive adhesive for a car interior sponge seat cushion.

Citation Information

Patent Citations

  • Preparation method of butyl rubber modified SIS hot-melt pressure-sensitive adhesive

    CN104650781A

  • Hot-melt adhesive for interior automotive trim

    JP2003327938A

Cited By

  • Hot-melt pressure-sensitive adhesive for mouse sticking board product and preparation method of hot-melt pressure-sensitive adhesive

    CN119684947A