Sealant and preparation method thereof
By using photothermal double curing sealants with epoxy resin and other materials in liquid crystal displays, the existing sealants are solved, and the efficient sealing and stable display of liquid crystal displays are achieved.
Patent Information
- Application Number
- CN202411138558.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-22
AI Technical Summary
In the use of existing sealants in liquid crystal displays, they have insufficient anti-water oxygen corrosion and impact resistance, resulting in poor display effect or failure of the device.
Using a combination of epoxy resin, diluent, photoinitiator, thermal initiator, filler and coupling agent, sealant is prepared through photothermal double curing reaction to ensure good adhesion between the sealant and the substrate, and has excellent Its resistance to water oxygen erosion and impact resistance.
It realizes effective sealing of the LCD screen, avoids water vapor and oxygen corrosion, improves the stability of the display effect and the weather resistance of the device, and has good impact resistance.
Smart Images

Figure BDA0005000080640000141 
Figure HDA0005000080650000011
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of adhesives, and in particular to a sealant and a preparation method thereof. Background Art
[0002] With the rapid development of digital production and life, LCD screens as digital windows are gaining more and more demand in various fields, such as new energy vehicles, chemical industry, medical equipment, consumer electronics, etc. The vigorous development of these fields has driven the growth of demand for LCD sealants. This is because LCD screens are sensitive to water vapor and oxygen. Once they are corroded by water vapor and oxygen, the display effect of the LCD screen will deteriorate, or even short-circuit and cause the device to fail and fail to work. Therefore, when the LCD screen is assembled and produced, a layer of sealant is needed on the frame to block the penetration of water vapor and oxygen.
[0003] However, the performance of current sealants cannot meet the requirements of use. Summary of the invention
[0004] In view of this, the present disclosure provides a sealant having good adhesion, impact resistance and water and oxygen corrosion resistance and a preparation method thereof.
[0005] To achieve the above objectives, the technical solution of the present disclosure is implemented as follows:
[0006] In a first aspect, the present disclosure provides a sealant, which includes, based on the total weight of the sealant: an epoxy resin, 15 to 20 wt%; a diluent, 6 to 15 wt%; a photoinitiator, 0.5 to 1.5 wt%; a thermal initiator, 0.1 to 0.2 wt%; a filler, 64 to 76 wt%; and a coupling agent, 0.2 to 0.3 wt%; wherein the epoxy resin includes an alicyclic epoxy resin and a bisphenol epoxy resin.
[0007] In some embodiments, based on the total weight of the epoxy resin, the content of the alicyclic epoxy resin is 55-75 wt %, and the content of the bisphenol epoxy resin is 25-45 wt %.
[0008] In some embodiments, the alicyclic epoxy resin is a diepoxy-functional alicyclic epoxy resin; the epoxy value of the alicyclic epoxy resin is 0.76 to 1; the bisphenol-type epoxy resin includes at least one of bisphenol A epoxy resin, bisphenol F epoxy resin and bisphenol S epoxy resin; the epoxy value of the bisphenol-type epoxy resin is 0.44 to 0.63.
[0009] In some embodiments, the photoinitiator includes a sulfonium-type cationic initiator.
[0010] In some embodiments, the thermal initiator comprises (pentafluoroethyl)trifluorophosphate.
[0011] In some embodiments, the coupling agent includes a silane coupling agent and / or a titanate coupling agent.
[0012] In some embodiments, the filler includes at least one of fumed silica, spherical silica, and talc.
[0013] In some embodiments, the diluent includes at least one of an oxetane monomer and an alicyclic epoxy group-containing methacrylate.
[0014] In some embodiments, the sealant further comprises: color powder; based on the total weight of the sealant, the content of the color powder is 0.005-0.01 wt %.
[0015] In a second aspect, the present disclosure provides a method for preparing the sealant in the above technical solution, the method comprising: mixing an epoxy resin, a diluent and a photoinitiator uniformly under light-proof and room temperature conditions to obtain a first mixture; adding a coupling agent and a filler to the first mixture, mixing uniformly under light-proof and room temperature conditions to obtain a second mixture; adding a thermal initiator to the second mixture, mixing uniformly under light-proof and room temperature conditions to obtain a third mixture; grinding the third mixture to obtain a sealant.
[0016] The present disclosure provides a sealant and a preparation method thereof. The sealant provided by the present disclosure includes an epoxy resin, a diluent, a photoinitiator, a thermal initiator, a filler and a coupling agent, and the epoxy resin includes an alicyclic epoxy resin and a bisphenol epoxy resin. The sealant is coated on a substrate and a curing reaction is performed by a light-heat dual curing method. The cured sealant has good adhesion to the substrate, and the cured sealant has good impact resistance and water-oxygen erosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The present invention provides a schematic flow chart of a method for preparing a sealant. DETAILED DESCRIPTION
[0018] The following will be combined with the embodiments of the present disclosure and the accompanying drawings to clearly and completely describe the technical solutions in the embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.
[0019] Throughout the specification, unless otherwise specifically stated, the terms used in the present disclosure should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used in the present disclosure have the same meanings as those generally understood by those skilled in the art to which the present disclosure belongs. In the event of a conflict, the present specification takes precedence.
[0020] The sealant used in liquid crystal display screens (also called "liquid crystal edge sealant") needs to have good sealing properties, water and oxygen corrosion resistance, weather resistance and chemical resistance, and protect the liquid crystal from leakage while not being affected by high temperature and high humidity. However, the sealant currently used in liquid crystal display screens is brittle and has poor crack and impact resistance.
[0021] In view of this, the present disclosure provides a sealant and a preparation method thereof.
[0022] The present invention provides a sealant, which comprises, based on the total weight of the sealant: 15-20 wt% of epoxy resin; 6-15 wt% of diluent; 0.5-1.5 wt% of photoinitiator; 0.1-0.2 wt% of thermal initiator; 64-76 wt% of filler; and 0.2-0.3 wt% of coupling agent; wherein the epoxy resin comprises alicyclic epoxy resin and bisphenol epoxy resin.
[0023] The term "epoxy resin" in this disclosure refers to an organic polymer compound containing two or more epoxy groups in the molecule. The molecular structure of epoxy resin is characterized by containing active epoxy groups in the molecular chain. The epoxy groups can be located at the end, in the middle or in a ring structure of the molecular chain. The epoxy resin can undergo a cross-linking reaction to form a three-dimensional network structure.
[0024] The term "alicyclic epoxy resin" in the present disclosure refers to an epoxy resin in which the epoxy group is located on an alicyclic ring. Compared with other epoxy resins, alicyclic epoxy resins have advantages such as high moisture and heat resistance and good weather resistance.
[0025] The term "bisphenol epoxy resin" in the present disclosure refers to an epoxy resin having a bisphenol group. Exemplarily, the bisphenol epoxy resin may include bisphenol A epoxy resin, bisphenol F epoxy resin or bisphenol S epoxy resin. Among them, bisphenol A epoxy resin can be prepared by reacting diphenol propane (i.e., bisphenol A) and epichlorohydrin, bisphenol F epoxy resin can be prepared by reacting 4,4'-dihydroxydiphenylmethane (i.e., bisphenol F) and epichlorohydrin, and bisphenol S epoxy resin can be prepared by reacting 4,4'-dihydroxydiphenyl sulfone (i.e., bisphenol S) and epichlorohydrin.
[0026] For example, the epoxy groups and hydroxyl groups in bisphenol A epoxy resin give the epoxy resin reactivity, making the epoxy resin have strong cohesion and adhesion; ether bonds and hydroxyl groups are polar groups, which help to improve wettability and adhesion; ether bonds and CC bonds make the macromolecules flexible; benzene rings give the polymer heat resistance and rigidity; isopropyl group reduces the intermolecular force and gives the resin a certain flexibility.
[0027] The term "diluent" in this disclosure refers to a compound used to adjust the viscosity of the system. The diluent can not only be used to reduce the viscosity of the adhesive, but also make the adhesive have good penetration and improve processing performance.
[0028] The term "photoinitiator" in the present disclosure refers to a compound that can absorb energy of a certain wavelength in the ultraviolet region (250-420nm) or the visible region (400-800nm) to generate free radicals, cations, etc., thereby initiating monomer polymerization, cross-linking and curing.
[0029] The term "thermal initiator" in the present disclosure refers to a compound that can generate free radicals under heating conditions, thereby initiating polymerization, cross-linking and curing of monomers.
[0030] The term "filler" in the present disclosure refers to a solid substance added to a sealant to improve the performance of the sealant and reduce the cost of the sealant.
[0031] The term "coupling agent" in the present disclosure refers to an additive used to improve the interfacial properties between resin and inorganic material. The coupling agent generally includes two parts, one part is inorganic-friendly and can interact with inorganic materials, and the other part is organic-friendly and can interact with resin. Therefore, the coupling agent can improve the interfacial interaction between organic and inorganic materials and improve the performance of the composite material.
[0032] The sealant provided by the present disclosure can be coated on a substrate and subjected to a photothermal dual curing reaction under ultraviolet light and heating conditions. The cured sealant has good adhesion to the substrate, and the cured sealant has good impact resistance and water and oxygen corrosion resistance. In some embodiments, the ultraviolet light energy range for the photothermal dual curing reaction of the sealant is 6000 to 8000 mJ / cm 2 ; The heating temperature range is 80~100℃.
[0033] The present disclosure has no particular limitation on the substrate coated with the sealant. For example, the substrate may include a liquid crystal display screen.
[0034] The sealant provided by the present invention includes epoxy resin, diluent, photoinitiator, thermal initiator, filler and coupling agent, and the epoxy resin includes alicyclic epoxy resin and bisphenol epoxy resin. The curing reaction is carried out by a dual curing method of light and heat. The cured sealant has good adhesion to the substrate, and the cured sealant has good impact resistance and water and oxygen erosion resistance.
[0035] The sealant provided by the present invention can be used as edge sealing glue for liquid crystal display screens, and has good adhesion to the liquid crystal display screens. Moreover, the sealant has excellent resistance to water and oxygen erosion, and can prevent water vapor and oxygen in the air from corroding the liquid crystal display screens, causing the display effect of the liquid crystal display screens to deteriorate, or even causing device failure due to a short circuit. In addition, the sealant has a certain degree of flexibility and exhibits excellent impact resistance, so that the sealant can remain stable in relatively extreme environments.
[0036] In some embodiments, the alicyclic epoxy resin is a diepoxy-functional alicyclic epoxy resin; the epoxy value of the alicyclic epoxy resin is 0.76-1.
[0037] For example, the alicyclic epoxy resin may include CELLOXIDE 2021P, whose chemical name is “3,4-epoxycyclohexylcarboxylic acid-3′,4′-epoxycyclohexyl methyl ester”; and CELLOXIDE 2081, whose chemical name is “ε-caprolactone-modified 3,4-epoxycyclohexylmethyl-3′,4′-epoxycyclohexylcarboxylate”.
[0038] Illustratively, the epoxy value of the alicyclic epoxy resin may be, for example, 0.80, 0.85, 0.90, or 0.95.
[0039] In some embodiments, the bisphenol epoxy resin includes at least one of bisphenol A epoxy resin, bisphenol F epoxy resin and bisphenol S epoxy resin; the epoxy value of the bisphenol epoxy resin is 0.44 to 0.63.
[0040] Illustratively, the bisphenol A type epoxy resin may include E42, E44 or E51.
[0041] Illustratively, the epoxy value of the bisphenol type epoxy resin is 0.46, 0.48, 0.50, 0.52, 0.54, 0.56, 0.58, 0.60 or 0.62.
[0042] In the sealant provided by the present disclosure, the epoxy resin is a mixture of alicyclic epoxy resin and bisphenol epoxy resin (for example, bisphenol A epoxy resin), the alicyclic epoxy resin provides better weather resistance and moisture and heat resistance, the bisphenol A epoxy resin provides better mechanical strength and bonding strength, the two types of epoxy resins complement each other, so that the cured sealant and the substrate have good adhesion, based on the good adhesion, the cured sealant has extremely high resistance to water and oxygen erosion and impact resistance. Compared with the sealant including a mixed system of acrylic resin and epoxy resin or acrylic modified epoxy resin, the sealant provided by the present disclosure has a smaller curing shrinkage, stronger heat and weather resistance, and higher bonding strength.
[0043] In some embodiments, based on the total weight of the epoxy resin, the content of the alicyclic epoxy resin is 55-75 wt %, and the content of the bisphenol epoxy resin is 25-45 wt %.
[0044] In some embodiments, the photoinitiator includes a sulfonium-type cationic initiator.
[0045] Exemplarily, the sulfonium type cationic initiator may include at least one of TR-PAG-201S, TR-PAG-202, TR-PAG-20102P, and TR-PAG-20108.
[0046] The photoinitiator with the trade name "TR-PAG-201S" has a chemical name of "mixed triphenyl sulfonium hexafluoroantimonate".
[0047] The photoinitiator with the trade name "TR-PAG-202" has a chemical name of "mixed triphenyl sulfonium hexafluorophosphate propylene carbonate solution".
[0048] The photoinitiator with the trade name "TR-PAG-20102P" has a chemical name of "diphenyl-(4-phenylthio)phenylthio hexafluoroantimonate".
[0049] The photoinitiator with the trade name "TR-PAG-20108" has a chemical name of "diphenyl-(4-phenylthio)phenylthiotetrakis(pentafluorophenyl)borate".
[0050] In some embodiments, the thermal initiator includes (pentafluoroethyl)trifluorophosphate.
[0051] Illustratively, the (pentafluoroethyl)trifluorophosphate includes at least one of TA-100 and IK-1.
[0052] The thermal initiator with the trade name "TA-100" has a chemical name of "diphenylsulfonium (pentafluoroethyl) trifluorophosphate".
[0053] The thermal initiator with the trade name "IK-1" has a chemical name of "diphenyliodonium (pentafluoroethyl) trifluorophosphate".
[0054] Compared with a single light curing or heat curing method, the sealant provided by the present invention adopts a dual light and heat curing method during use, and the curing reaction is more complete. The cured sealant has good adhesion to the substrate, which helps to improve the sealant's impact resistance and water and oxygen erosion resistance, and has better sealing properties for the substrate.
[0055] In some embodiments, the coupling agent includes a silane coupling agent and / or a titanate coupling agent.
[0056] Exemplarily, the silane coupling agent includes at least one of KH-550, KH-560, and KH-570.
[0057] Here, KH-550 refers to γ-aminopropyltriethoxysilane; KH-560 refers to γ-glycidoxypropyltrimethoxysilane; and KH-570 refers to γ-(methacryloyloxy)propyltrimethoxysilane.
[0058] Exemplarily, the titanate coupling agent includes at least one of TCA-AA75, TCA-TE, and TCA-DC.
[0059] The coupling agent with the trade name "TCA-AA75" has a chemical name of "bis(acetylacetonate) diisopropyl titanate".
[0060] The coupling agent with the trade name "TCA-TE" has a chemical name of "bistriethanolamine diisopropyl titanate".
[0061] The coupling agent with the trade name "TCA-DC" has a chemical name of "bis(ethyl acetoacetate) titanate diisopropyl".
[0062] The sealant provided by the present disclosure may include only a silane coupling agent or a titanate coupling agent, or may include both a silane coupling agent and a titanate coupling agent, which is more helpful in improving the adhesion between the cured sealant and the substrate, and further helps to improve the impact resistance and water and oxygen erosion resistance of the sealant.
[0063] In some embodiments, the filler includes at least one of fumed silica, spherical silica, and talc.
[0064] The sealant provided by the present disclosure has good adhesion between the sealant and the substrate, and adding a suitable amount of filler can further improve the isolation effect of water vapor and oxygen.
[0065] In some embodiments, the diluent includes at least one of an oxetane monomer and an alicyclic epoxy group-containing methacrylate.
[0066] Exemplarily, the diluent may include at least one of TCM218, TCM207, TCM203, TCM109, TCM201, and M100.
[0067] The diluent with the trade name "TCM218" has a chemical name of "3-ethyl-3-[4-[(3-ethyloxetane-3-yl)methoxy]butoxymethyl]oxetane".
[0068] The diluent with the trade name "TCM207" has the chemical name "3-ethyl-3-[(oxyethylene-2-methoxy)methyl]oxetane".
[0069] The diluent with the trade name "TCM203" has the chemical name "1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene".
[0070] The diluent with the trade name "TCM109" has the chemical name "3-ethyl-3-[(2-ethylhexyloxy)methyl]oxetane".
[0071] The diluent with the trade name "TCM201" has the chemical name "3,3'-(oxybismethylene)-bis-(3-ethyl)-oxetane".
[0072] For example, the diluent may include M100, which is methacrylate containing alicyclic epoxy groups.
[0073] In some embodiments, the sealant further comprises: color powder; based on the total weight of the sealant, the content of the color powder is 0.005-0.01 wt %.
[0074] Here, the sealant may further include a toner for adjusting the appearance color of the sealant. Exemplarily, the toner may include carbon black. In fact, the present disclosure does not specifically limit the color of the toner included in the sealant, and a suitable toner may be selected according to actual needs.
[0075] refer to Figure 1 , Figure 1 The schematic diagram of the process for preparing the sealant provided by the present disclosure is as follows. Figure 1 As shown, the present disclosure also provides a method for preparing a sealant, the method comprising:
[0076] Step S101: Mix epoxy resin, diluent and photoinitiator uniformly under light-proof and room temperature conditions to obtain a first mixture.
[0077] Step S102: adding a coupling agent and a filler to the first mixture, and mixing them evenly under the condition of being protected from light and at room temperature to obtain a second mixture.
[0078] Step S103: adding a thermal initiator to the second mixture, and mixing the mixture evenly under the condition of being protected from light and at room temperature to obtain a third mixture;
[0079] Step S104: grinding the third mixture to obtain a sealant.
[0080] In the above technical solution, in step S101, epoxy resin, diluent and photoinitiator are mixed evenly to obtain a first mixture; in step S102, the first mixture, coupling agent and filler are mixed evenly to obtain a second mixture; in step S103, the second mixture and thermal initiator are mixed evenly. Appropriate stirring can be performed for uniform mixing, and the present disclosure has no special restrictions on the stirring speed and stirring time.
[0081] Here, since the addition of diluent in step S101 can reduce the viscosity of the system, a higher speed can be used for stirring in step S101. However, since the addition of filler in step S102 causes greater resistance to stirring, a lower speed can be used for stirring in step S102.
[0082] In a specific embodiment, in step S101, stirring can be performed at 600 rpm for 1 hour in a dark environment and at room temperature; in step S102, stirring can be performed at 600 rpm for 1 hour in a dark environment and at room temperature; in step S103, stirring can be performed at 100 rpm for 1 hour in a dark environment and at room temperature.
[0083] It should be noted that, considering that the sealant provided in the present disclosure is a light-heat dual-curing sealant, in the process of preparing the sealant, after adding the photoinitiator in step S010, the entire preparation process needs to be protected from light, for example, the mixing process of the first mixture, the second mixture and the third mixture is carried out in a light-proof tank.
[0084] Optionally, step S102 includes: adding a coupling agent, a filler and a color powder to the first mixture, and mixing them uniformly under light-proof conditions and at room temperature to obtain a second mixture.
[0085] Optionally, the second mixture may be allowed to stand for a period of time after stopping stirring, and then the thermal initiator may be added and mixed evenly.
[0086] Optionally, the third mixture is ground and dispersed using a three-roll mill, and the sealant can be obtained after vacuum degassing.
[0087] Here, since stirring is performed in step S101, step S102 and step S103 to ensure uniform mixing, bubbles may be introduced into the system, a vacuum environment is created, and the bubbles in the system are squeezed out by using the pressure difference.
[0088] Hereinafter, embodiments of the present disclosure are described. The embodiments described below are exemplary and are only used to explain the present disclosure, and should not be construed as limiting the present disclosure. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in the art or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0089] Among the epoxy resins used below, alicyclic epoxy resins CELLOXIDE 2021P and CELLOXIDE 2081 were purchased from Daicel Corporation. Bisphenol A epoxy resins E51 and E44 were purchased from Wuxi Qianguang Chemical Raw Materials Co., Ltd.; bisphenol F epoxy resin NPEF-170 was purchased from Nanya Plastics Industry Co., Ltd. Epoxy acrylic resin L-6111 was purchased from Lancolu.
[0090] Among the diluents used below, diluents TCM207, TCM201, TCM218 and TCM109 were all purchased from Changzhou Qiangli Electronic New Materials Co., Ltd.; diluent M100 was purchased from Daicel Corporation.
[0091] Among the thermal initiators used below, thermal initiator TA-100 was purchased from Sanya Pro Co., Ltd., and thermal initiator IK-1 was purchased from Sanya Pro Co., Ltd.
[0092] Among the photoinitiators used below, photoinitiators TR-PAG-201S, TR-PAG-202, and TR-PAG-20108 were all purchased from Changzhou Qiangli Electronic New Materials Co., Ltd.
[0093] Among the coupling agents used below, silane coupling agents KH-560 and KH-570 were purchased from Nanjing Nengde New Material Technology Co., Ltd. Titanate coupling agents TCA-AA75, TCA-TE and TCA-DC were purchased from Changzhou Qiangli Electronic New Materials Co., Ltd.
[0094] Among the fillers used below, fumed silica, 5 μm silica and 1 μm silica were all purchased from Cabot Corporation of the United States.
[0095] Among the toners used below, B4 carbon black was purchased from Orion Corporation.
[0096] Example 1
[0097] (1) 26.6 g of alicyclic epoxy resin CELLOXIDE 2021P, 10 g of bisphenol A epoxy resin E51, 2 g of photoinitiator TR-PAG-201S, 10 g of diluent TCM201 and 17.8 g of diluent TCM207 were added to a light-proof stirring tank and stirred at 600 rpm for 1 h at room temperature.
[0098] (2) Then, 0.2 g of silane coupling agent KH-560 and 0.2 g of titanate coupling agent TCA-AA75, 2 g of fumed silica M5, 100.8 g of 5 μm spherical silica and 20 g of 1 μm spherical silica and 0.01 g of toner B4 carbon black were added to (1) in sequence, and the mixture was stirred for 3 h at room temperature in the dark.
[0099] (3) After stopping stirring for 30 minutes, 0.2 g of thermal initiator TA-100 was added to (2) and stirred at 100 rpm for 1 hour at room temperature.
[0100] (4) The mixture in (3) was fully ground using a three-roll mill, and then vacuum degassed for 20 minutes to obtain a sealant.
[0101] Example 2
[0102] (1) 20 g of alicyclic epoxy resin CELLOXIDE 2021P, 9.6 g of bisphenol F type epoxy resin NPEF170, 1 g of photoinitiator TR-PAG-202, 10 g of diluent M100 and 7.8 g of diluent TCM201 were added to a light-proof stirring tank and stirred at 500 rpm for 1 h at room temperature.
[0103] (2) Then, 0.3 g of silane coupling agent KH-570, 0.2 g of titanate coupling agent TCA-TE, 2 g of fumed silica M5, 65 g of 5 μm spherical silica, 50.8 g of 1 μm spherical silica and 0.01 g of toner B4 carbon black were added to (1) in sequence, and the mixture was stirred for 4 h at room temperature in the dark.
[0104] (3) After stopping stirring for 30 minutes, 0.3 g of thermal initiator TA-100 was added to (2) and stirred at 100 rpm for 1 hour at room temperature.
[0105] (4) The mixture in (3) was fully ground using a three-roll mill, and then vacuum degassed for 30 minutes to obtain a sealant.
[0106] Example 3
[0107] (1) 14.6 g of alicyclic epoxy resin CELLOXIDE 2081, 12 g of bisphenol A epoxy resin E44, 1.5 g of photoinitiator TR-PAG-20108, 5 g of diluent TCM218 and 5.5 g of diluent TCM109 were added to a light-proof stirring tank and stirred at 600 rpm for 1 h at room temperature.
[0108] (2) Then, 0.22 g of silane coupling agent KH-560 and 0.22 g of titanate coupling agent TCA-DC, 2 g of fumed silica A200, 80.4 g of 5 μm spherical silica and 40.4 g of 1 μm spherical silica and 0.01 g of toner B4 carbon black were added to (1) in sequence, and the mixture was stirred for 4 h at room temperature in the dark.
[0109] (3) After stopping stirring for 30 minutes, 0.2 g of thermal initiator IK-1 was added to (2), and stirred at 100 rpm for 2 hours at room temperature.
[0110] (4) The mixture in (3) was fully ground using a three-roll mill, and then vacuum degassed for 30 minutes to obtain a sealant.
[0111] Comparative Example 1
[0112] (1) 36.6 g of alicyclic epoxy resin CELLOXIDE 2021P, 2 g of photoinitiator TR-PAG-201S, 10 g of diluent M100 and 17.8 g of diluent TCM207 were added to a light-proof stirring tank and stirred at 600 rpm for 1 h at room temperature.
[0113] (2) Then, 0.2 g of silane coupling agent KH-560 and 0.2 g of titanate coupling agent TCA-AA75, 2 g of fumed silica M5, 100.8 g of 5 μm spherical silica and 20 g of 1 μm spherical silica and 0.01 g of toner B4 carbon black were added to (1) in sequence, and stirring was continued at room temperature in the dark for 3 h.
[0114] (3) After stopping stirring for 30 minutes, 0.2 g of thermal initiator TA-100 was added to (2) and stirred at 100 rpm for 1 hour at room temperature.
[0115] (4) The mixture in (3) was fully ground using a three-roll mill, and then vacuum degassed for 20 minutes to obtain a sealant.
[0116] Comparative Example 2
[0117] (1) 36.6 g of bisphenol A epoxy resin E51, 2 g of photoinitiator TR-PAG-201S, 10 g of diluent M100 and 17.8 g of diluent TCM207 were added to a light-proof stirring tank and stirred at 600 rpm for 1 h at room temperature.
[0118] (2) Then, 0.2 g of silane coupling agent KH-560 and 0.2 g of titanate coupling agent TCA-AA75, 2 g of fumed silica M5, 100.8 g of 5 μm spherical silica and 20 g of 1 μm spherical silica and 0.01 g of toner B4 carbon black were added to (1) in sequence, and the mixture was stirred for 3 h at room temperature in the dark.
[0119] (3) After stopping stirring for 30 minutes, 0.2 g of thermal initiator TA-100 was added to (2) and stirred at 100 rpm for 1 hour at room temperature.
[0120] (4) The mixture in (3) was fully ground using a three-roll mill, and then vacuum degassed for 30 minutes to obtain a sealant.
[0121] Comparative Example 3
[0122] (1) 36.6 g of epoxy acrylic resin L-6111, 2 g of photoinitiator TR-PAG-201S, 10 g of diluent M100 and 17.8 g of diluent TCM207 were added to a light-proof stirring tank and stirred at 600 rpm for 1 h at room temperature.
[0123] (2) Then, 0.2 g of silane coupling agent KH-560 and 0.2 g of titanate coupling agent TCA-AA75, 2 g of fumed silica M5, 100.8 g of 5 μm spherical silica and 20 g of 1 μm spherical silica and 0.01 g of toner B4 carbon black were added to (1) in sequence, and the mixture was stirred for 3 h at room temperature in the dark.
[0124] (3) After stopping stirring for 30 minutes, 0.2 g of thermal initiator TA-100 was added to (2) and stirred at 100 rpm for 1 hour at room temperature.
[0125] (4) The mixture in (3) was fully ground using a three-roll mill, and then vacuum degassed for 30 minutes to obtain a sealant.
[0126] Comparative Example 4
[0127] (1) 26.6 g of alicyclic epoxy resin CELLOXIDE 2021P, 10 g of bisphenol A epoxy resin E51, 2 g of photoinitiator TR-PAG-201S, 10 g of diluent M100 and 17.8 g of diluent TCM207 were added to a light-proof stirring tank and stirred at 600 rpm for 1 h at room temperature.
[0128] (2) Then, 0.2 g of silane coupling agent KH-560 and 0.2 g of titanate coupling agent TCA-AA75, 2 g of fumed silica M5, 100.8 g of 5 μm spherical silica and 20 g of 1 μm spherical silica and 0.01 g of toner B4 carbon black were added to (1) in sequence, and the mixture was stirred for 3 h at room temperature in the dark.
[0129] (3) The mixture in (2) was fully ground using a three-roll mill, and then vacuum degassed for 20 minutes to obtain a sealant.
[0130] Comparative Example 5
[0131] (1) 26.6 g of alicyclic epoxy resin CELLOXIDE 2021P, 10 g of bisphenol A epoxy resin E51, 2 g of photoinitiator TR-PAG-201S, 10 g of diluent M100 and 17.8 g of diluent TCM207 were added to a light-proof stirring tank and stirred at 600 rpm for 1 h at room temperature.
[0132] (2) Then, 2 g of fumed silica M5, 100.8 g of 5 μm spherical silica, 20 g of 1 μm spherical silica and 0.01 g of toner B4 carbon black were added to (1) in sequence, and stirring was continued at room temperature in the dark for 3 h.
[0133] (3) After stopping stirring for 30 minutes, 0.2 g of thermal initiator TA-100 was added to (2) and stirred at 100 rpm for 1 hour at room temperature.
[0134] (4) The mixture in (3) was fully ground using a three-roll mill, and then vacuum degassed for 20 minutes to obtain a sealant.
[0135] Comparative Example 6
[0136] (1) 26.6 g of alicyclic epoxy resin CELLOXIDE 2021P, 10 g of bisphenol A epoxy resin E51, 2 g of photoinitiator TR-PAG-201S, 10 g of diluent M100 and 17.8 g of diluent TCM207 were added to a light-proof stirring tank and stirred at 600 rpm for 1 h at room temperature.
[0137] (2) Then, 0.2 g of silane coupling agent KH-560, 0.2 g of titanate coupling agent TCA-AA75, 2 g of fumed silica M5, 50.4 g of 5 μm spherical silica, 10 g of 1 μm spherical silica and 0.01 g of toner B4 carbon black were added to (1) in sequence, and the mixture was stirred for 3 h at room temperature in the dark.
[0138] (3) After stopping stirring for 30 minutes, 0.2 g of thermal initiator TA-100 was added to (2) and stirred at 100 rpm for 1 hour at room temperature.
[0139] (4) The mixture in (3) was fully ground using a three-roll mill, and then vacuum degassed for 20 minutes to obtain a sealant.
[0140] Test Example 1: Shear force test
[0141] Use a dispensing machine to drop a drop of sealant on a 5mm*5mm*1mm glass sheet, with a needle inner diameter of 0.42mm, and then press a glass sheet of the same size on the glue, making the width of the glue strip 2mm and the thickness of the glue 80-150μm. Use 6000mJ / cm 2The glass pieces were exposed to UV light and baked at 80℃ for 1 hour to cure the sealant. The glass pieces after the sealant was cured were tested with a push-pull tester (manufacturer: Deruiyin Precision Technology Co., Ltd., model: MFM1200) to test the thrust of the glass sliding, and the shear force at 25℃ and 121℃.
[0142] Test Example 2: Water Vapor Transmission Rate Test
[0143] A 100*100*1 mm film was produced, and after curing, it was tested using a water vapor transmission rate tester (manufacturer: Labthink, model: W3 / 031) at a condition of 50° C. and 95% RH.
[0144] Test Example 3: Saturated Steam Test
[0145] The electronic devices sealed with the sealants provided in the embodiments and comparative examples were placed in a high-pressure accelerated aging test chamber (manufacturer: AP-PCT-40F) and tested at 121°C and 100% RH for 168 hours to test whether the electronic devices could continue to work normally.
[0146] Test Example 4: Impact Test
[0147] The liquid crystal display screen sealed with the sealant provided in each embodiment and comparative example was subjected to impact test. The test instrument was a high sampling impact measuring instrument (model VENZO 640H). The test conditions were that the impact pulse type was a half-sine wave and the acceleration was 500m / s. 2 , duration is 6ms, the number of impacts is 10 times in each test direction, and the number of test directions is not less than 6.
[0148] The test results of various embodiments and comparative examples are shown in Table 1.
[0149] Table 1 Summary of test results of embodiments and comparative examples
[0150]
[0151] The shear force test in Test Example 1 can be used to characterize the adhesion between the sealant and the substrate. The water vapor transmission rate test in Test Example 2 and the saturated steam test in Test Example 3 can be used to characterize the moisture and heat resistance and weather resistance of the sealant. The impact test in Test Example 4 can be used to characterize the impact resistance of the sealant.
[0152] The sealants provided in Examples 1 to 3 have good adhesion to the substrate after the curing reaction, and the cured sealants have good impact resistance and water and oxygen corrosion resistance.
[0153] The sealant provided in Comparative Example 1 does not contain bisphenol A epoxy resin, and its adhesion to the substrate is poor, it does not have good waterproof properties and has poor impact resistance. The sealant provided in Comparative Example 2 does not contain alicyclic epoxy resin, has a high water vapor permeability, and has poor moisture and heat resistance. The sealant provided in Comparative Example 3 uses epoxy acrylic resin instead of epoxy resin, and its moisture and heat resistance and impact resistance are not ideal. The sealant provided in Comparative Example 4 only uses a photoinitiator, which is a single light-curing sealant. Its shear force is low, and its moisture and heat resistance and impact resistance are poor. The sealant provided in Comparative Example 5 does not contain a coupling agent, and its shear force decreases, and its impact resistance decreases. The amount of spherical silica filler in the sealant provided in Comparative Example 6 is halved, and its ability to block water vapor is significantly weakened.
[0154] The above description is only a preferred embodiment of the present disclosure, and does not limit the patent scope of the present disclosure. All equivalent structural changes made by using the contents of the present disclosure and the drawings under the inventive concept of the present disclosure, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present disclosure.
Claims
1. A sealant, characterized in that: Based on the total weight of the sealant, the sealant comprises: Epoxy resin, 15-20wt%; Diluent, 6-15wt%; Photoinitiator, 0.5-1.5wt%; Thermal initiator, 0.1-0.2 wt%; Filler, 64-76 wt %; and Coupling agent, 0.2-0.3wt%; wherein the epoxy resin includes alicyclic epoxy resin and bisphenol epoxy resin.
2. The sealant according to claim 1, characterized in that: Based on the total weight of the epoxy resin, the content of the alicyclic epoxy resin is 55-75wt%, and the content of the bisphenol epoxy resin is 25-45wt%.
3. The sealant according to claim 1, characterized in that: The alicyclic epoxy resin is a diepoxy functional alicyclic epoxy resin; the epoxide value of the alicyclic epoxy resin is 0.76 to 1; The bisphenol epoxy resin includes at least one of bisphenol A epoxy resin, bisphenol F epoxy resin and bisphenol S epoxy resin; the epoxy value of the bisphenol epoxy resin is 0.44-0.
63.
4. The sealant according to claim 1, characterized in that: The photoinitiator includes a sulfonium type cationic initiator.
5. The sealant according to claim 1, characterized in that: The thermal initiator includes (pentafluoroethyl) trifluorophosphate.
6. The sealant according to claim 1, characterized in that: The coupling agent includes a silane coupling agent and / or a titanate coupling agent.
7. The sealant according to claim 1, characterized in that: The filler includes at least one of fumed silica, spherical silica and talc.
8. The sealant according to claim 1, characterized in that: The diluent includes at least one of an oxetane monomer and an alicyclic epoxy group-containing methacrylate.
9. The sealant according to claim 1, characterized in that: The sealant further comprises: color powder; based on the total weight of the sealant, the content of the color powder is 0.005-0.01wt%.
10. A method for preparing a sealant as claimed in any one of claims 1 to 9, characterized in that: The method comprises: Mixing epoxy resin, diluent and photoinitiator uniformly under light-proof and room temperature conditions to obtain a first mixture; Adding a coupling agent and a filler to the first mixture, and mixing them uniformly under the condition of being protected from light and at room temperature, to obtain a second mixture; Adding a thermal initiator to the second mixture, and mixing the mixture evenly under the condition of being protected from light and at room temperature, to obtain a third mixture; The third mixture is ground to obtain a sealant.