Method for separating rare earth and iron
Fe3+ is reduced to Fe2+ by chemical reduction method, and valence state regulation is carried out before rare earth extraction, which solves the problem of poor separation effect between rare earth and iron, achieves good separation between rare earth and iron, and improves the purity of rare earth products.
Patent Information
- Application Number
- CN202411120715.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the separation effect of rare earths and iron is poor, especially when Fe3+ is present in the rare earth solution, the selective extraction of iron by the extractant leads to a decrease in the purity of the rare earth product.
Chemical reduction method is used to reduce Fe3+ to Fe2+ and then extract, which avoids the trivalent selective extraction of iron by the extraction agent, thereby achieving good separation between rare earths and iron.
The Fe3+ valence state was regulated by chemical reduction method before extracting rare earth ions, and the trivalent selective extraction of iron was successfully avoided, which achieved good separation effect between rare earth and iron, and improved the purity of rare earth products.
Smart Images

Figure CN118996174A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrometallurgy, and in particular relates to a method for separating rare earth and iron. Background Art
[0002] Rare earth is an important strategic resource widely used in many fields such as catalysis, hydrogen storage, optical fiber, communication and gas separation. However, ensuring the purity of rare earth products is a prerequisite for their application, and even trace impurities may lead to performance degradation.
[0003] There are many types of rare earth minerals, such as bastnaesite, ionic rare earth ores and mixed rare earth ores. Iron is an impurity with a relatively high content. The current wet smelting and separation technology of rare earth ores mainly includes acid roasting, leaching and extraction separation processes. There is a relatively high content of Fe in the rare earth leachate. 3+ From the extraction point of view, Fe 3+ It is a very easy-to-extract component, which is easily extracted by various types of extractants and often enters the organic phase before other metals. The commonly used organic phosphine extractants for extracting rare earth ions are very sensitive to Fe 3+ It also has strong selectivity, so the presence of iron greatly interferes with the separation of rare earth elements.
[0004] In the methods for recovering rare earth and iron disclosed in patents such as CN116676486A and CN115161499A, iron is first extracted by using an extractant to obtain an iron-rich organic phase and a rare earth raffinate, thereby separating rare earth and iron. 3+ With RE 3+ (Rare earth ions) are all trivalent, and the extractant has the problem of selective extraction according to the valence state, resulting in the problem of simultaneous extraction, and the separation effect of rare earth and iron is not good. CN106801154A discloses a method for removing iron impurities in metal praseodymium by solvent extraction, and the synergistic effect of extractants DPDOMA, DPDDdDGA and DBDDdDGA on Pr is excellent, and the separation of Pr and Fe is achieved. The essence of this method is still a traditional extraction process and is not universal.
[0005] Therefore, based on the shortcomings of the prior art, a method for separating rare earth and iron needs to be provided. Summary of the invention
[0006] The purpose of the present invention is to provide a method for separating rare earth and iron, and to solve the problem of Fe 3+ In the presence of iron, it interferes with the extraction of rare earths and achieves a good separation effect of rare earths and iron.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] The present invention provides a method for separating rare earth and iron, the method comprising the following steps:
[0009] (1) The Fe in the rare earth iron mixed solution is reduced by chemical reduction 3+ A reduction reaction occurs to obtain a reduced solution;
[0010] (2) extracting the reduction solution obtained in step (1) with an extracting liquid to obtain a rare earth-rich organic phase and an iron-rich raffinate.
[0011] In rare earth ion-containing solution systems such as rare earth oxide acid leaching solution and / or ionic rare earth ore leaching solution, there is often a high content of Fe 3+ Impurity ions are easily extracted simultaneously with the extraction of rare earth ions, thereby affecting the purity of the rare earth product. The present invention adopts a reduction method to firstly reduce Fe 3+ To regulate the valence state and reduce it to Fe 2 + Then, the rare earth ions are extracted, which avoids the selective extraction of iron in the trivalent state by the extractant, thereby achieving a good separation effect of rare earth and iron.
[0012] In the present invention, the reduction reaction process mainly involves the following reactions:
[0013]
[0014] In the present invention, the organic phosphoric acid exists in the form of a dimer (H2A2) in the organic phase. When the dimer dissociates into monomers, acidic ionization occurs at the interface to generate an extractant by an ion exchange mechanism. The main extraction process is as follows:
[0015]
[0016] RE 3+ +3H2A2=RE(HA2)3+3H +
[0017] Preferably, the rare earth iron mixed solution comprises rare earth oxide acid leaching solution and / or ionic rare earth ore leaching solution.
[0018] Preferably, the concentration of rare earth ions in the rare earth iron mixed solution is 10-10000 ppm, for example, it can be 10 ppm, 100 ppm, 500 ppm, 1000 ppm, 5000 ppm or 10000 ppm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] Preferably, in the rare earth iron mixed solution, the mass concentration ratio of rare earth ions to iron ions is 3+ / Fe 3+The value is 1-1000, for example, 1, 5, 10, 50, 100, 500 or 1000, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Preferably, the pH of the rare earth iron mixed solution is <7, for example, it can be 0, 1, 2, 3, 4, 5, 6 or 6.5, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0021] Preferably, the chemical reduction method includes photocatalytic reduction, electrochemical reduction or the use of a reducing agent.
[0022] Preferably, the reducing agent comprises an organic reducing agent and / or an inorganic reducing agent.
[0023] Preferably, the organic reducing agent comprises ascorbic acid and / or oxalic acid.
[0024] Preferably, the inorganic reducing agent comprises nitrite and / or thiosulfate.
[0025] Preferably, the amount of the reducing agent is Fe 3+ 1-200 times the amount of the substance, for example, 1 time, 5 times, 10 times, 50 times, 100 times, 150 times or 200 times, but not limited to the listed values, other unlisted values within the numerical range are also applicable, preferably 1-100 times.
[0026] Preferably, the reduction reaction time is 0.5-2 h, for example, 0.5 h, 1 h, 1.5 h or 2 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0027] Preferably, the temperature of the reduction reaction is 15-100°C, for example, it can be 15°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 20-80°C.
[0028] Preferably, the concentration of the extractant in the extract is 0.01-100%, for example, it can be 0.01%, 0.1%, 1%, 10%, 30%, 50%, 80% or 100%, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 0.1-80%.
[0029] Preferably, the extractant in the extract comprises an organophosphorus extractant.
[0030] Preferably, the organophosphorus extractant comprises any one or a combination of at least two of P507 (2-ethylhexyl 2-ethylhexyl phosphate), P204 (di(2-ethylhexyl) phosphate), TBP (tributyl phosphate), P350 (dimethylheptyl methylphosphonate), Cyanex 923 (straight chain trialkylphosphine oxide), Cyanex 272 (bis(2,4,4-trimethylpentyl)phosphonic acid), N235 (trioctyldecyl tertiary amine), DDPA (didecylphosphinic acid) or DEHPA (dialkyl phosphate). Typical but non-limiting combinations include a combination of P507 and P204, a combination of TBP and P350, a combination of P350 and Cyanex 923, a combination of TBP and DEHPA, a combination of P507, P204 and Cyanex 923, or a combination of P507, Cyanex 272, DEHPA and TBP.
[0031] Preferably, the extract comprises an extractant and a diluent.
[0032] Preferably, the diluent includes any one or a combination of at least two of benzene, chloroform, carbon tetrachloride, n-hexane, n-heptane, n-dodecane, n-butyl ether, kerosene or ethyl acetate, and typical but non-limiting combinations include a combination of benzene and chloroform, a combination of carbon tetrachloride and n-hexane, a combination of n-dodecane and n-butyl ether, a combination of kerosene and ethyl acetate, a combination of benzene, chloroform and carbon tetrachloride. Or, a combination of n-dodecane, n-butyl ether, kerosene and ethyl acetate.
[0033] Preferably, the extraction ratio O / A is (1-50):(10-1), for example, it can be 1:10, 1:5, 1:1, 30:10, 30:5, 30:1, 50:10, 50:5 or 50:1, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably (1-30):(10-1).
[0034] Preferably, the extraction stage is 1-100, for example, it can be 1, 5, 10, 30, 50, 80 or 100, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] The present invention adopts chemical reduction method to firstly reduce Fe before extracting rare earth ions. 3+ To regulate the valence state and reduce it to Fe 2+ Then, the rare earth ions are extracted, which avoids the selective extraction of iron in the trivalent state by the extractant, thereby achieving a good separation effect of rare earth and iron. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a process flow chart of the method provided in Example 1;
[0038] Figure 2 is an extraction result diagram of the method provided in Example 1;
[0039] Figure 3 This is a diagram of the extraction results of the method provided in Example 2. DETAILED DESCRIPTION
[0040] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0041] Example 1
[0042] This embodiment provides a Figure 1 The method for separating rare earths and iron is shown.
[0043] The rare earth iron mixed solution used is erbium iron mixed solution, Er 3+ The concentration is 1000ppm, Fe 3+ The concentration is 10 ppm, the pH of the solution is 1.7, and the concentration ratio of rare earth ions to iron ions is 100.
[0044] The method comprises the following steps:
[0045] (1) Weigh 30 mL of rare earth iron mixed solution, add 0.012 g of ascorbic acid, the purity of ascorbic acid is 99.7%, and the ascorbic acid and Fe 3+ The molar ratio of the substance is 12:1, and the reaction is carried out for 1 hour to obtain a reduction solution;
[0046] (2) Take 10 mL of the reducing solution obtained in step (1), add 10 mL of an extracting solution, wherein the extracting agent is P507, the concentration is 0.01 mol / L (equivalent to a volume fraction of 2.5%), and the diluent is n-heptane, shake at room temperature of 25°C for 40 min for extraction, and then separate the organic phase and the raffinate, and subsequently the organic phase is stripped and concentrated to obtain a rare earth sample.
[0047] The concentrations of erbium and iron in the obtained raffinate were analyzed to be 6.2 ppm and 6.8 ppm, respectively. The extraction rates of erbium and iron were 99.4% and 24.7%, respectively. The separation coefficient β was 497.0.
[0048] Example 2
[0049] This embodiment provides a method for separating rare earth and iron.
[0050] The rare earth iron mixed solution used is erbium iron mixed solution, Er 3+ The concentration of Fe is 10138ppm, 3+ The concentration is 9.6 ppm, the pH of the solution is 1.5, and the concentration ratio of rare earth ions to iron ions is 1000.
[0051] The method comprises the following steps:
[0052] (1) Weigh 30 mL of rare earth iron mixed solution, add 0.012 g of ascorbic acid, the purity of ascorbic acid is 99.7%, and the ascorbic acid and Fe 3+ The molar ratio of the substance is 12:1, and the reaction is carried out for 1 hour to obtain a reduction solution;
[0053] (2) Take 10 mL of the reducing solution obtained in step (1), add 10 mL of an extracting solution, wherein the extracting agent is P507 with a volume fraction of 15%, and the diluent is n-heptane, shake at room temperature of 25° C. for 40 min for extraction, and then separate the organic phase and the raffinate. Subsequently, the organic phase is stripped and concentrated to obtain a rare earth sample.
[0054] The concentrations of erbium and iron in the obtained raffinate were analyzed to be 1349 ppm and 9.11 ppm, respectively. The extraction rates of erbium and iron were 86.7% and 5.1%, respectively. The separation coefficient β was 121.1.
[0055] Example 3
[0056] This embodiment provides a method for separating rare earth and iron.
[0057] The rare earth iron mixed solution used is erbium iron mixed solution, Er 3+ The concentration of Fe is 10011ppm, 3+ The concentration is 10.8 ppm, the pH of the solution is 2, and the concentration ratio of rare earth ions to iron ions is about 1000.
[0058] The method comprises the following steps:
[0059] (1) Weigh 30 mL of rare earth iron mixed solution, add 0.001 g of ascorbic acid, the purity of ascorbic acid is 99.7%, and the ascorbic acid and Fe 3+ The molar ratio of the substance is 1, and the reaction is carried out for 0.5h to obtain a reduction solution;
[0060] (2) Take 10 mL of the reducing solution obtained in step (1), add 100 mL of an extracting solution, wherein the extracting agent is P507 with a volume fraction of 0.1%, and the diluent is n-heptane, shake for 40 min at room temperature of 25° C. for extraction, and then separate the organic phase and the raffinate. Subsequently, the organic phase is stripped and concentrated to obtain a rare earth sample.
[0061] The concentrations of erbium and iron in the obtained raffinate were analyzed to be 5400 ppm and 10.28 ppm, respectively. The extraction rates of erbium and iron were 51.0% and 4.9%, respectively. The separation coefficient β was 18.
[0062] Example 4
[0063] This embodiment provides a method for separating rare earth and iron.
[0064] The rare earth iron mixed solution used is erbium iron mixed solution, Er 3+ The concentration is 10000ppm, Fe 3+ The concentration is 10 ppm, the pH of the solution is 1.8, and the concentration ratio of rare earth ions to iron ions is about 1000.
[0065] The method comprises the following steps:
[0066] (1) Weigh 30 mL of rare earth iron mixed solution, add 0.1 g of ascorbic acid, the purity of ascorbic acid is 99.7%, and the ascorbic acid and Fe 3+ The molar ratio of the substance is 200, and the reaction is carried out for 0.5h to obtain a reduction solution;
[0067] (2) Take 30 mL of the reducing solution obtained in step (1), add 1 mL of an extracting solution, wherein the extracting agent is P507 with a volume fraction of 2.5%, and the diluent is n-heptane, shake at room temperature of 25° C. for 40 min for extraction, and then separate the organic phase and the raffinate. Subsequently, the organic phase is stripped and concentrated to obtain a rare earth sample.
[0068] The concentrations of erbium and iron in the obtained raffinate were analyzed to be 6150 ppm and 10.25 ppm, respectively. The extraction rates of erbium and iron were 44.1% and 2.4%, respectively. The separation coefficient β was 32.3.
[0069] Example 5
[0070] This embodiment provides a method for separating rare earth and iron.
[0071] The rare earth iron mixed solution used is the same as that in Example 2.
[0072] Compared with Example 2, the method is the same as Example 2 except that the amount of ascorbic acid and other substances in step (1) is replaced by oxalic acid.
[0073] Example 6
[0074] This embodiment provides a method for separating rare earth and iron.
[0075] The rare earth iron mixed solution used is the same as that in Example 2.
[0076] Compared with Example 2, the method is the same as Example 2 except that the amount of ascorbic acid and other substances in step (1) is replaced by iron powder.
[0077] Example 7
[0078] This embodiment provides a method for separating rare earth and iron.
[0079] The rare earth iron mixed solution used is the same as that in Example 2.
[0080] Compared with Example 2, the method is the same as Example 2 except that the amount of ascorbic acid and other substances in step (1) is replaced by sodium nitrite.
[0081] Comparative Example 1
[0082] This comparative example provides a method for separating rare earth and iron, and the rare earth iron mixed solution used is the same as that in Example 2.
[0083] Compared with Example 2, the method does not perform step (1), and the rest is the same as Example 2.
[0084] The concentrations of rare earth elements and iron in the reducing solution and the obtained raffinate in the examples and comparative examples were determined by ICP-OES method, and the element extraction rate was calculated. The formula for calculating the separation coefficient β between rare earth and iron is as follows:
[0085] The separation coefficient (β) is defined as the ratio of the distribution ratios (D) of the two elements and is calculated as follows:
[0086] D RE =C org / C aq
[0087] D Fe =C' org / C' aq
[0088] β RE / Fe =D RE / D Fe
[0089] In the formula, C org , C aq are the concentrations of rare earth elements in the loaded organic phase and the residual water phase (mol / L); C' org , C' aq are the concentrations of Fe in the loaded organic phase and the residual water phase (mol / L), respectively.
[0090] Figure 2 and Figure 3 The figure is a bar graph showing the concentrations in the reducing solution and the raffinate before and after extraction in Example 1 and Example 2.
[0091] The calculation results of the embodiments and comparative examples are listed in Table 1.
[0092] Table 1
[0093]
[0094] As can be seen from Table 1, the chemical reduction method provided in the present application can effectively separate rare earth ions and iron ions, especially when the concentration ratio of rare earth ions to iron ions in the solution is large (RE 3+ / Fe 3+ ≥100) and low iron ion concentration (10-100ppm), also have good separation effect, and significant effect is achieved by using ascorbic acid as reducing agent.
[0095] In Example 6 and Example 7, iron powder and sodium nitrite were used as reducing agents, and the reducing effect was reduced, and other impurity ions were introduced into the solution at the same time.
[0096] In summary, the present invention adopts a chemical reduction method to firstly reduce Fe 3+ To regulate the valence state and reduce it to Fe 2+ Then, the rare earth ions are extracted, which avoids the selective extraction of iron in the trivalent state by the extractant, thereby achieving a good separation effect of rare earth and iron.
[0097] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for separating rare earth and iron, characterized in that: The method comprises the following steps: (1) The Fe in the rare earth iron mixed solution is reduced by chemical reduction 3+ A reduction reaction occurs to obtain a reduced solution; (2) extracting the reduction solution obtained in step (1) with an extracting liquid to obtain a rare earth-rich organic phase and an iron-rich raffinate.
2. The method according to claim 1, characterized in that: The rare earth iron mixed solution includes rare earth oxide acid leaching solution and / or ionic rare earth ore leaching solution; Preferably, the concentration of rare earth ions in the rare earth iron mixed solution is 10-10000 ppm; Preferably, in the rare earth iron mixed solution, the mass concentration ratio of rare earth ions to iron ions is 3+ / Fe 3+ 1-1000; Preferably, the pH of the rare earth iron mixed solution is <7.
3. The method according to claim 1 or 2, characterized in that: The chemical reduction method includes photocatalytic reduction, electrochemical reduction or the use of a reducing agent.
4. The method according to claim 3, characterized in that The reducing agent includes an organic reducing agent and / or an inorganic reducing agent; Preferably, the organic reducing agent comprises ascorbic acid and / or oxalic acid; Preferably, the inorganic reducing agent includes any one of nitrite or thiosulfate or a combination of at least two of them.
5. The method according to claim 3 or 4, characterized in that: The amount of the reducing agent is Fe 3+ 1-200 times, preferably 1-100 times, the amount of the substance.
6. The method according to any one of claims 1 to 5, characterized in that: The reduction reaction time is 0.5-2h; Preferably, the temperature of the reduction reaction is 15-100°C, preferably 20-80°C.
7. The method according to any one of claims 1 to 6, characterized in that: The concentration of the extractant in the extract is 0.01-100%, preferably 0.1-80%; Preferably, the extractant in the extract comprises an organophosphorus extractant; Preferably, the organophosphorus extractant comprises any one of P507, P204, TBP, P350, Cyanex 923, Cyanex 272, N235, DDPA or DEHPA, or a combination of at least two thereof.
8. The method according to any one of claims 1 to 7, characterized in that: The extract comprises an extractant and a diluent; Preferably, the diluent comprises any one or a combination of at least two of benzene, chloroform, carbon tetrachloride, n-hexane, n-heptane, n-dodecane, n-butyl ether, kerosene or ethyl acetate.
9. The method according to any one of claims 1 to 8, characterized in that: The extraction phase ratio O / A is (1-50):(10-1), preferably (1-30):(10-1).
10. The method according to any one of claims 1 to 9, characterized in that: The extraction stages are 1-100.
Citation Information
Patent Citations
Liquid-liquid-liquid three-phase extraction and separation method of enriched iron in middle phase
CN102212685A
Method for removing metal ion purity of rare earth aqueous solution extraction
CN103468950A
Electric reduction-P extraction and separation process to recover RE and Co from wast Nd-Fe-B material
CN1441070A
Cited By
Rare earth extracting agent and application method thereof
CN120026195A
A rare earth extractant and its application method
CN120026195B
Method for electrolytically removing trace iron and aluminum from rare earth solution by using rotary porous cathode
CN122235777A